AC 43-4B Corrosion Control for Aircraft

This AC provides guidance to aircraft operators and maintenance, repair, and overhaul (MRO) organizations for the development of a corrosion control program. This AC applies to Title 14 of the Code of Federal Regulations (14 CFR) parts 121, 129, and 135 operators. This AC is a summary of the current available data regarding identification and treatment of corrosive attack on aircraft structures and engine materials. Corrosion inspection frequency, corrosion identification, and especially corrosion treatment continues to be the responsibility of the operator. These inspections should be accomplished per this AC, the manufacturer’s recommendations, or the operator’s own maintenance program. The procedures in this AC are an acceptable means, but not the only acceptable means, of corrosion treatment. The information in this AC is applicable to aircraft for which the manufacturer has not published corrosion control information. Where the airframe or engine manufacturer has published a recommended corrosion inspection schedule and treatment program, the applicable program must take precedence over the recommendation of this AC. The contents of this document do not have the force and effect of law and are not meant to bind the public in any way, and the document is intended only to provide information to the public regarding existing requirements under the law or agency policies. This AC is intended for use by persons performing maintenance, alteration, or preventive maintenance on aircraft, engines, propellers, or appliances in accordance with 14 CFR part 43.

Official source ↗ Open PDF

U.S. Department of Transportation Federal Aviation Administration

Advisory Circular

Subject: Corrosion Control for Aircraft Date: 9/11/18 AC No: 43-4B Initiated by: AFS-300 Change:

This advisory circular (AC) is a summary of the current available data regarding identification and treatment of corrosive attack on aircraft structures and engine materials. Corrosion inspection frequency, corrosion identification, and especially corrosion treatment continues to be the responsibility of the operator. These inspections should be accomplished per this AC, the manufacturer’s recommendations, or the operator’s own maintenance program. The procedures in this AC are an acceptable means, but not the only acceptable means, of corrosion treatment. The information in this AC is applicable to aircraft for which the manufacturer has not published corrosion control information. Where the airframe or engine manufacturer has published a recommended corrosion inspection schedule and treatment program, the applicable program must take precedence over the recommendation of this AC. The contents of this document do not have the force and effect of law and are not meant to bind the public in any way. This document is intended only to provide clarity to the public regarding existing requirements under the law or agency policies.

Rick Domingo Executive Director, Flight Standards Service

ii

CONTENTS Paragraph Page

Chapter 1. General … 1-1

1.1 Purpose of This Advisory Circular (AC) … 1-1

1.2 Audience … 1-1

1.3 Where You Can Find This AC … 1-1

1.4 What This AC Cancels … 1-1

1.5 Related Reading Material … 1-1

1.6 Background … 1-1

1.7 Catastrophic Corrosion Events … 1-2

1.8 Corrosion Control Program … 1-2

1.9 AC Feedback Form … 1-3

1.10–1.99 Reserved … 1-3

Chapter 2. Corrosion Theory … 2-1

2.1 Introduction … 2-1

2.2 Background … 2-1

2.3 Development of Corrosion … 2-2

2.4 Factors Influencing Corrosion … 2-2

2.5 Forms of Corrosion … 2-4

2.6 Corrosion and Mechanical Factors … 2-10

2.7 Common Corrosive Agents … 2-14

2.8 Microorganisms … 2-16

2.9 Metallic Mercury Corrosion on Aluminum Alloys … 2-17

2.10–2.99 Reserved … 2-17

Chapter 3. Effects of Corrosion … 3-1

3.1 General … 3-1

3.2 Effects of Corrosion on Metals … 3-1

3.3–3.99 Reserved … 3-5

Chapter 4. Corrosion-Prone Areas and Preventive Maintenance … 4-1

4.1 General … 4-1

4.2 Exhaust Trail Areas … 4-1

4.3 Battery Compartments and Battery Vent Openings … 4-1

iii

4.4 Lavatories, Buffets, Galleys, Doorways, and Cockpit Floorboards … 4-2

4.5 Bilge Areas … 4-2

4.6 Wheel Wells and Landing Gear … 4-2

4.7 External Skin Areas … 4-5

4.8 Water Entrapment Areas … 4-9

4.9 Engine Frontal Areas and Cooling Air Vents … 4-9

4.10 Electronic Package Compartments … 4-11

4.11 Miscellaneous Trouble Areas … 4-12

4.12 Factors in Corrosion Control … 4-17

4.13 Preventive Maintenance … 4-21

4.14–4.99 Reserved … 4-35

Chapter 5. Inspection Requirements … 5-1

5.1 General … 5-1

5.2 Frequency of Inspections … 5-1

5.3 Recommended Depth of Inspection … 5-2

5.4 Primary Approach … 5-3

5.5–5.99 Reserved … 5-13

Chapter 6. Corrosion Removal Techniques … 6-1

Section 1. Safety Procedures … 6-1

6.1 General … 6-1

6.2 General Corrosion Control Work Procedures … 6-4

6.3–6.9 Reserved … 6-4

Section 2. Corrosion Removal Techniques … 6-5

6.10 General … 6-5

6.11 Standard Methods … 6-5

6.12 Preparations for Rework … 6-5

6.13 Paint Removal … 6-6

6.14 Special Techniques … 6-6

6.15 Fairing or Blending Reworked Areas … 6-7

6.16 Chemical Testing … 6-13

6.17 Chemical Spot Analysis of Magnetic Metals … 6-14

iv

6.18 Chemical Spot Analysis of Nonmagnetic Metals … 6-15

6.19 Surface Treatment Testing … 6-16

6.20 Post-Identification Cleaning and Refinishing … 6-17

6.21–6.25 Reserved … 6-17

Section 3. Mechanical Corrosion Removal by Blasting … 6-18

6.26 General … 6-18

6.27 Safety Precautions … 6-18

6.28–6.39 Reserved … 6-18

Section 4. Corrosion Damage and Rework Limits … 6-19

6.40 Discussion … 6-19

6.41 Removal of Corrosion … 6-20

6.42 Determining Degree of Corrosion Damage … 6-21

6.43 Determining Rework Limits … 6-21

6.44 Determining Material Thickness Reduction After Corrosion Cleanup … 6-21

6.45–6.49 Reserved … 6-22

Section 5. Aluminum and Aluminum Alloys … 6-23

6.50 Treatment … 6-23

6.51 Processing of Aluminum Surfaces … 6-23

6.52 Repair of Aluminum Alloy Sheet Metal … 6-27

6.53 Corrosion Removal Around Countersunk Fasteners in Aluminum Alloy … 6-28

6.54 Examples of Removing Corrosion from Aluminum and Aluminum Alloys … 6-28

6.55–6.59 Reserved … 6-30

Section 6. Magnesium Alloys … 6-31

6.60 Treatment of Wrought Magnesium Sheets and Forgings … 6-31

6.61 Repair of Magnesium Sheet Metal After Extensive Corrosion Removal … 6-31

6.62 In-Place Treatment of Magnesium Castings … 6-31

6.63 Example of Removing Corrosion from Magnesium … 6-32

6.64–6.69 Reserved … 6-34

Section 7. Ferrous Metals … 6-35

6.70 General … 6-35

6.71 Mechanical Removal of Iron Rust … 6-35

v

6.72 Chemical Surface Treatment of Steel Surfaces … 6-36

6.73 Removal of Corrosive Products from High-Stressed Steel Parts … 6-37

6.74 Special Treatment of Stainless Steel Alloys … 6-37

6.75 Example of Process for Removal of Corrosion from Steel Parts … 6-37

6.76–6.79 Reserved … 6-38

Section 8. Plated Parts … 6-39

6.80 Chromium and Nickel Plated Parts … 6-39

6.81 Cadmium and Zinc Plated Parts … 6-39

6.82–6.89 Reserved … 6-39

Section 9. Other Metals and Alloys … 6-40

6.90 Noble Metal Coatings—Cleanup and Restoration … 6-40

6.91 Copper and Copper Alloys … 6-40

6.92 Titanium Alloys … 6-40

6.93–6.99 Reserved … 6-41

Chapter 7. Special Problems … 7-1

7.1 Mercury Spills/Corrosion Damage … 7-1

7.2 Corrosion Protection for Agricultural Aircraft … 7-3

7.3–7.99 Reserved … 7-4

List of Figures

Figure 2-1. Simplified Corrosion Cell Showing Conditions which Must Exist for

Electrochemical Corrosion … 2-1

Figure 2-2. Elimination of Corrosion by Application of an Organic Film to Metal Surface .... 2-2

Figure 2-3. Uniform Etch Corrosion … 2-4

Figure 2-4. Pitting Corrosion … 2-5

Figure 2-5. Galvanic Corrosion of Magnesium Adjacent to Steel Fastener … 2-5

Figure 2-6. Concentration Cell Corrosion … 2-7

Figure 2-7. Intergranular Cracking and Corrosion on a Wing Spar Chord … 2-7

Figure 2-8. Severe Exfoliation Corrosion of a Seat Track … 2-8

Figure 2-9. Severe Exfoliation Corrosion … 2-8

Figure 2-10. Filiform Corrosion … 2-9

Figure 2-11. Filiform Corrosion Before and After Paint Removal … 2-10

Figure 2-12. Stress-Corrosion Cracking of 7079-T6 Fitting … 2-11

vi

Figure 2-13. Stress-Corrosion Cracking Starting at a Pit in CRES Material … 2-12

Figure 2-14. Stress-Corrosion Cracking of an Extruded Section … 2-12

Figure 2-15. Fretting Corrosion and Cracking from Cyclic Loading of Lug … 2-13

Figure 4-1. Exhaust Trail Area Corrosion Control Points … 4-1

Figure 4-2. Typical Damage to Floor Around Lavatories, Buffets, and Galleys … 4-2

Figure 4-3. Landing Gear and Wheel Corrosion Points … 4-4

Figure 4-4. Intergranular Corrosion of 7075-T6 Aluminum Adjacent to Steel Fastener … 4-5

Figure 4-5. Crack and Skin Bulging Caused by Corrosion … 4-6

Figure 4-6. Spot-Welded Skin Corrosion … 4-7

Figure 4-7. Hinge Corrosion Points … 4-8

Figure 4-8. Hinge Failure Caused by Corrosion … 4-8

Figure 4-9. Reciprocating Engine Frontal Area Corrosion … 4-10

Figure 4-10. Jet Engine Frontal Area Corrosion Points … 4-11

Figure 4-11. Spar Chord Lifting Caused by Corrosion Products … 4-15

Figure 4-12. Skin Bulging Around Fasteners … 4-15

Figure 4-13. Opening of a Corroded Lap Joint for Repair … 4-16

Figure 4-14. Close-Up View of a Corroded Lap Joint … 4-16

Figure 4-15. North America Corrosion Severity Map … 4-22

Figure 4-16. South America Corrosion Severity Map … 4-23

Figure 4-17. Africa Corrosion Severity Map … 4-24

Figure 4-18. South Pacific Corrosion Severity Map … 4-25

Figure 4-19. Asia Corrosion Severity Map … 4-26

Figure 4-20. Europe and Asia Minor Corrosion Severity Map … 4-27

Figure 4-21. Blocked Drain Passages Resulted in Accumulation of Corrosion

Contaminates and Moisture … 4-28

Figure 5-1. Corrosion Found After Removing Cargo Door Threshold Covers … 5-2

Figure 5-2. Corrosion Under Chipped and Loose Paint on Wing Skin … 5-4

Figure 5-3. Corrosion Indicated by Blistering of Paint in Fuel Cell … 5-4

Figure 5-4. Popped Rivet Heads Resulting from Corrosion Products … 5-5

Figure 5-5. Skin Bulging Around Fasteners Caused by Pressure from Corrosion Products … 5-5

Figure 5-6. Corrosion Cracking Between Fasteners on a Wing Spar … 5-6

Figure 5-7. Faying Surface Corrosion on Wing Spar Chord with Corrosion Cracking

Also Visible … 5-6

vii

Figure 5-8. Severe Crown Stringer Corrosion … 5-7

Figure 5-9. Spar Chord Corrosion … 5-7

Figure 5-10. Removal of Fillet Seal from Internal Edge of Lap Joint Exposed Full Extent

of Corrosion … 5-8

Figure 5-11. Removal of Insulation Blankets Exposed Corrosion … 5-8

Figure 5-12. Corrosion Developed Under Leveling Compound Installed During Previous

Repair of Overwing Exit … 5-9

Figure 5-13. Corrosion Behind a Structural Component on a Wing Spar … 5-9

Figure 5-14. Severely Corroded Lap Joint … 5-10

Figure 5-15. Severely Corroded Lap Joint … 5-10

Figure 5-16. Local Paint Removal Required to Expose Full Extent of Corrosion … 5-11

Figure 5-17. Corroded Area After Paint Removal from Wing Skin … 5-11

Figure 5-18. Bonderite 1200 Treatment Prior to Painting May Highlight Presence of

Remaining Corrosion or Cracks … 5-12

Figure 6-1. Blendout of Corrosion as Single Depression Width … 6-9

Figure 6-2. Typical Example of Acceptable Cleanup of Corrosion Pits … 6-10

Figure 6-3. Blendout of Multiple Pits in Corroded Area … 6-10

Figure 6-4. Profile of Reworked Corroded Areas in Regions of Limited Access … 6-11

Figure 6-5. Steel Particles from Fasteners or Nutplates May Cause Future Corrosion

Problems in Aluminum Structure … 6-11

Figure 6-6. Incomplete Removal of Corrosion Products Resulted in Reoccurrence

of Corrosion … 6-12

Figure 6-7. Incomplete Removal of Corrosion Products Resulted in Reoccurrence

of Corrosion … 6-12

Figure 6-8. Severe Corrosion Requiring Trimming Out of Damaged Area … 6-20

Figure 6-9. Corrosion at Fastener Holes Removed by Spot Facing … 6-20

Figure 6-10. Corrosion Damage and Rework Measurement Using Depth Dial Gauge … 6-22

Figure 6-11. Removing Oil and Surface Dirt … 6-24

Figure 6-12. Polishing and Brightening Alclad Surfaces … 6-24

Figure 6-13. Cleaning and Stripping Paint … 6-25

Figure 6-14. Cleaning and Inhibiting Corroded Aluminum Surfaces … 6-26

Figure 6-15. Removing Excess Inhibitor Solution … 6-27

Figure 6-16. Applying Wax to Cleaned Surfaces … 6-27

viii

Figure 6-17. Removing Corrosion Products from Ordinary Steel Surfaces … 6-36

Figure 6-18. Removing Corrosion Products from Highly Stressed Steel Parts … 6-36

List of Tables

Table 3-1. Corrosion of Metals … 3-4

Table 4-1. Galvanic Series of Metals and Alloys … 4-19

Table 4-2. Grouping of Metals and Alloys … 4-20

Table 6-1. Abrasives for Corrosion Removal … 6-8

CHAPTER 1. GENERAL › 1.6 Background.

CHAPTER 1. GENERAL

1.1 Purpose of This Advisory Circular (AC). This AC provides guidance to aircraft operators and maintenance, repair, and overhaul (MRO) organizations for the development of a corrosion control program. This AC applies to Title 14 of the Code of Federal Regulations (14 CFR) parts 121, 129, and 135 operators. This AC is a summary of the current available data regarding identification and treatment of corrosive attack on aircraft structures and engine materials. Corrosion inspection frequency, corrosion identification, and especially corrosion treatment continues to be the responsibility of the operator. These inspections should be accomplished per this AC, the manufacturer’s recommendations, or the operator’s own maintenance program. The procedures in this AC are an acceptable means, but not the only acceptable means, of corrosion treatment. The information in this AC is applicable to aircraft for which the manufacturer has not published corrosion control information. Where the airframe or engine manufacturer has published a recommended corrosion inspection schedule and treatment program, the applicable program must take precedence over the recommendation of this AC. The contents of this document do not have the force and effect of law and are not meant to bind the public in any way, and the document is intended only to provide information to the public regarding existing requirements under the law or agency policies. This AC is intended for use by persons performing maintenance, alteration, or preventive maintenance on aircraft, engines, propellers, or appliances in accordance with 14 CFR part 43.

1.2 Audience. This AC applies to aircraft operators and MRO organizations.

1.3 Where You Can Find This AC. You can find this AC on the Federal Aviation Administration’s (FAA) website at https://www.faa.gov/regulations_policies/advisory_cir culars and the Dynamic Regulatory System (DRS) at https://drs.faa.gov.

1.4 What This AC Cancels. AC 43-4A, Corrosion Control for Aircraft, dated July 25, 1991, is canceled.

1.5 Related Reading Material.

1.5.1 FAA Documents (current editions). AC 65-15, Airframe and Powerplant Mechanics Airframe Handbook. You can find this AC at https://www.faa.gov/regulations_policies/a dvisory_circulars.

1.5.2 Other Documents:

• Naval Air Systems Command, NAVAIR 01-1A-509-1, Cleaning and Corrosion Control.

• U.S. Air Force Technical Order TO 1-1-691, Cleaning and Corrosion Prevention and Control, Aerospace and Non-Aerospace Equipment.

1.6 Background. Corrosion is the electrochemical deterioration of a metal because of its chemical reaction with a surrounding environment. While the aerospace industry is

1.8 Corrosion Control Program. › 1.8.2 Operators must follow a constant cycle of cleaning, inspection,…

continuously developing new and better materials, progress is offset partly by a more aggressive operational environment and by the complexity of the corrosion phenomenon, which can take many different forms. The resistance of aircraft materials to corrosion can drastically change with only a small environmental change.

1.7 Catastrophic Corrosion Events. Corrosion is most often a slow process of material deterioration, taking place over a long period of time. Examples are general corrosion, pitting, stress-corrosion cracking, environmental embrittlement, and corrosion fatigue and exfoliation. Corrosion degradation can occur very quickly, in days or even hours, and with catastrophic results. Corrosion thrives on both the chemical and mechanical aspects of the environment and can cause catastrophic structural failure without warning.

1.8 Corrosion Control Program.

1.8.1 The possibility of an in-flight mishap or excessive down time for structural repairs mandates an active Corrosion Prevention and Control Program (CPCP). The operational environment of the aircraft sets the type and aggressiveness of the program. Aircraft exposed to such environments as salt air, heavy atmospheric industrial pollution, or over-water operations, will need a more stringent CPCP than an aircraft operating in a dry environment.

1.8.2 Operators must follow a constant cycle of cleaning, inspection, operational preservation, and lubrication to prevent corrosion. Prompt detection and removal of corrosion will limit the extent of damage to an aircraft and its components. The basic philosophy of a CPCP should consist of:

1. Personnel adequately trained in recognizing corrosion, including conditions, detection and identification, cleaning, treating, and preservation;

2. Thorough knowledge of corrosion identification techniques;

3. Proper emphasis on the concept of all-hands responsibility for corrosion control;

4. Scheduled corrosion inspections;

5. Aircraft washing at regularly scheduled intervals;

6. Routine cleaning or wipe down of all exposed unpainted surfaces;

7. Keeping drain holes and passages open and functional;

8. Scheduled inspections, removals, and reapplications of preservation compounds;

9. Early detection and repair of damaged protective coatings;

10. Periodic thorough cleaning, lubrication, and preservation;

11. Prompt corrosion treatment after detection;

12. Accurate recordkeeping and reporting of material or design deficiencies; and

13. Use of appropriate materials, equipment, and technical publications.

CHAPTER 1. GENERAL › 1.10–1.99. RESERVED.

1.9 AC Feedback Form. For your convenience, the AC Feedback Form is the last page of this AC. Note any deficiencies found, clarifications needed, or suggested improvements regarding the contents of this AC on the Feedback Form.

1.10–1.99. RESERVED.

CHAPTER 2. CORROSION THEORY

2.1 Introduction. This chapter introduces corrosion theory, causes of corrosion, factors influencing its development, and descriptions of forms of corrosion and common corrosive agents.

2.2 Background. › 2.2.2 Elimination of any one of these conditions will stop corrosion.

2.2 Background.

2.2.1 Corrosion is a natural phenomenon which attacks metal by chemical or electrochemical action and converts it into a metallic compound, such as an oxide, hydroxide, or sulfate. Corrosion is different from erosion, which causes destruction by mechanical action. The corrosion occurs because metals tend to return to their natural state. Noble metals, such as gold and platinum, do not corrode since they are chemically uncombined in their natural state. Four conditions must exist before corrosion can occur (see Figure 2-1, Simplified Corrosion Cell Showing Conditions which Must Exist for Electrochemical Corrosion):

1. Presence of an anode, or a metal that will corrode;

2. Presence of a cathode, a dissimilar conductive material which has less tendency to corrode;

3. Presence of an electrolyte, a conductive liquid; and

4. Electrical contact between the anode and cathode, which is usually by metal-to-metal contact, or through a fastener.

Figure 2-1. Simplified Corrosion Cell Showing Conditions which Must Exist for

Electrochemical Corrosion

2.2.2 Elimination of any one of these conditions will stop corrosion. An example would be a paint film on the metal surface (see Figure 2-2, Elimination of Corrosion by Application of an Organic Film to Metal Surface). Metals such as stainless steel and titanium can produce corrosion products so tightly bound to the corroding metal that they form an

2.4 Factors Influencing Corrosion. › 2.4.1 Some factors which influence metal corrosion and the rate of…

invisible oxide, or passive, film, preventing further corrosion. When a film of corrosion products is loose and porous, such as those of aluminum and magnesium, an electrolyte can easily penetrate and continue the corrosion process, producing more extensive damage than surface appearance would show.

Figure 2-2. Elimination of Corrosion by Application of an Organic Film to Metal Surface

2.3 Development of Corrosion.

2.3.1 All corrosive attack begins on the surface of the metal, and the corrosion process involves two chemical changes: 1) the metal that is attacked or oxidized undergoes an anodic change, and 2) the corrosive agent is reduced or undergoes a cathodic change. The tendency of most metals to corrode creates one of the major problems in aircraft maintenance, particularly where adverse environmental or weather conditions exist.

2.3.2 Paint coatings can mask initial stages of corrosion. Since corrosion products occupy more volume than the original metal, paint surfaces should be inspected often for such irregularities as blisters, flakes, chips, and lumps.

2.4 Factors Influencing Corrosion.

2.4.1 Some factors which influence metal corrosion and the rate of corrosion are the:

1. Type of metal;

2. Heat treatment and grain direction;

3. Presence of a dissimilar, less corrodible metal (galvanic corrosion);

4. Anode and cathode surface areas (in galvanic corrosion);

2.4 Factors Influencing Corrosion. › 2.4.8 In some cases, corrosion progresses at the same rate no matter…

5. Temperature;

6. Presence of electrolytes (such as hard water, saltwater, or battery fluids);

7. Availability of oxygen;

8. Presence of different concentrations of the same electrolyte;

9. Presence of biological organisms;

10. Mechanical stress on the corroding metal;

11. Time of exposure to a corrosive environment; and

12. Lavatory fluids with hard water, saltwater, or battery fluids.

2.4.2 Most pure metals are not suitable for aircraft construction and are used to form alloys. Most alloys are made up entirely of small, crystalline regions called grains. Corrosion can occur on the less resistant surfaces of these regions and at boundaries between regions, resulting in the formation of pits and intergranular corrosion. Metals have a wide range of corrosion resistance. The most chemically active metals (which tend to lose electrons easily, such as magnesium and aluminum) corrode easily. The most noble metals (which do not lose electrons easily, such as gold and silver) do not corrode easily.

2.4.3 High-temperature environments accelerate corrosion by increasing chemical reaction rates and moisture content in saturated air.

2.4.4 Electrolytes, or electrically conducting solutions, form when condensation, salt spray, rain, or rinse water accumulate on surfaces. Dirt, salt, acidic gases, and engine exhaust gases can dissolve on wet surfaces, increasing electrolyte conductivity and also the rate of corrosion.

2.4.5 When areas such as between faying surfaces or in deep crevices partially confine an electrolyte on a metal surface, that surface corrodes more rapidly than other metal surfaces outside this area. This area of corrosion is called an oxygen concentration cell. The reduced oxygen content of the confined electrolyte causes adjacent metal to become anodic to other metal surfaces immersed in electrolyte and exposed to air on the same part.

2.4.6 Slimes, molds, fungi, and other living organisms, some of which are microscopic, can grow on damp surfaces. The area where such organisms become established tends to remain damp, increasing the possibility of corrosion.

2.4.7 Manufacturing processes, such as machining, forming, welding, or heat treatment, can leave stresses in aircraft parts. This residual stress can cause cracking in a corrosive environment when the threshold for stress-corrosion is exceeded.

2.4.8 In some cases, corrosion progresses at the same rate no matter how long the metal has been exposed to an environment. In other cases, corrosion can decrease with time because of a barrier formed by corrosion products, or increase with time if a barrier is breaking down.

2.5 Forms of Corrosion. › 2.5.2 Pitting Corrosion.

2.5 Forms of Corrosion. Different types of corrosive attack will vary with the metal concerned, corrosive media location, and the length of time of exposure. For descriptive purposes, the types are listed under what the FAA considers the most commonly accepted titles.

2.5.1 Uniform Etch Corrosion. Uniform etch corrosion results from a direct chemical attack on a metal surface and involves only the metal surface (see Figure 2-3, Uniform Etch Corrosion). On a polished surface, this type of corrosion may first appear as a general dulling of the surface. If the attack continues, the surface becomes rough and possibly frosted in appearance. However, it should be noted that the discoloration or general dulling of metal created by exposure to elevated temperatures is not uniform etch corrosion.

2.5.2 Pitting Corrosion. This is the most common effect of corrosion on aluminum and magnesium alloys, but can occur in other metal alloys (see Figure 2-4, Pitting Corrosion). It is first noticeable as a white or gray powdery deposit, similar to dust, which blotches the surface. When the deposit is cleaned away, tiny pits or holes in the surface can be seen. The combination of small active anodes and large passive cathodes causes severe pitting. The principle also applies to metals passivated by chemical treatments or environmental condition.

Figure 2-3. Uniform Etch Corrosion

2.5 Forms of Corrosion. › 2.5.3 Galvanic Corrosion.

Figure 2-4. Pitting Corrosion

2.5.3 Galvanic Corrosion. This corrosion type occurs when two dissimilar metals make electrical contact in the presence of an electrolyte (see Figure 2-5, Galvanic Corrosion of Magnesium Adjacent to Steel Fastener). The rate of corrosion depends on differences in reaction activity between dissimilar metals. The greater the difference, the faster corrosion occurs. For example, aluminum skin panels and stainless steel doublers, riveted together in an aircraft wing, form a galvanic couple if moisture and contamination are present. The rate of galvanic corrosion also depends on the size of the parts in contact. If the surface area of the corroding metal (the anode) is smaller than the surface area of the less active metal (the cathode), corrosion will be rapid and severe. But if the corroding metal is larger than the less active metal, corrosion will be slow and superficial.

Figure 2-5. Galvanic Corrosion of Magnesium Adjacent to Steel Fastener

2.5 Forms of Corrosion. › 2.5.5 Intergranular Corrosion.

2.5.4 Concentration Cell Corrosion or Crevice Corrosion. In this type, corrosion occurs in either a metal-to-metal joint, at the edge of a joint of identical metals, or on a spot on the metal surface covered by a foreign material (see Figure 2-6, Concentration Cell Corrosion). Below is a discussion on the three general types of concentration cell corrosion:

2.5.4.1 Metal Ion Concentration Cells. A liquid solution that may consist of water and ions of a metal in contact with water. A high concentration of the metal ions will normally exist under faying surfaces where the solution is stagnant. A low concentration of metal ions will exist adjacent to the crevice created by the faying surface. An electrical potential will exist between the two points of connection, and the area of the metal in contact with the low concentration of metal ions will be anodic and will corrode. The area in contact with the high metal ion concentration will be cathodic and will not show signs of corrosion. Figure 2-6 illustrates metal ion concentration cell corrosion.

2.5.4.2 Oxygen Concentration Cells. A solution in contact with a metal surface that normally contains dissolved oxygen. An oxygen cell can develop at any point where oxygen in the air does not diffuse into the solution, and creates a difference in oxygen concentration between two points where the solution and metal meet. Typical locations of oxygen concentration cells are under: 1) either metallic or nonmetallic deposits on the metal surface, 2) faying surfaces such as riveted lap joints, or 3) gaskets, wood, rubber, and other materials in contact with the metal surface. Corrosion will occur at the area of low oxygen concentration (the anode), as Figure 2-6 illustrates. Alloys such as stainless steel, which owe their corrosion resistance to surface passivity, are particularly susceptible to this type of crevice corrosion.

2.5.4.3 Active-Passive Cells. Metals which depend on a tightly adhering passive film, like an oxide for corrosion protection such as on corrosion resistant steel (CRES), are prone to rapid corrosive attack by active-passive cells. Corrosive action usually starts as an oxygen concentration cell. As an example, salt deposits on the metal surface in the presence of water containing oxygen can create the oxygen cell. The passive film will be broken beneath a dirt particle. Once the passive film is broken, corrosion will attack the active metal beneath the film. An electrical potential will develop between the large area of the cathode, or passive film, and the small area of the anode, or active metal, and rapid pitting of the active metal will result, as shown in Figure 2-6.

2.5.5 Intergranular Corrosion. This corrosion attacks grain boundaries of a metal. Each grain has a clearly defined boundary which differs chemically from the metal within the grain center. The grain boundary and grain center can react with each other as anode and cathode when in contact with an electrolyte. Rapid selective corrosion at the grain boundary can occur and cause delamination (see Figure 2-7, Intergranular Cracking and Corrosion on a Wing Spar Chord). High-strength aluminum alloys, such as schedule 2014 or 7075, are more susceptible to intergranular corrosion if improperly heat-treated then exposed to a corrosive environment.

2.5 Forms of Corrosion. › 2.5.6 Exfoliation Corrosion.

Figure 2-6. Concentration Cell Corrosion

Figure 2-7. Intergranular Cracking and Corrosion on a Wing Spar Chord

2.5.6 Exfoliation Corrosion. Exfoliation is an advanced form of intergranular corrosion where the surface grains of a metal are lifted up by the force of expanding corrosion products occurring at the grain boundaries. The lifting up or swelling is visible evidence of exfoliation corrosion. Exfoliation occurs on extruded, rolled, wrought, and forged high-strength aluminum and magnesium parts. See Figures 2-8, Severe Exfoliation Corrosion of a Seat Track, and 2-9, Severe Exfoliation Corrosion.

Figure 2-8. Severe Exfoliation Corrosion of a Seat Track

Figure 2-9. Severe Exfoliation Corrosion

2.5 Forms of Corrosion. › 2.5.7 Filiform Corrosion.

2.5.7 Filiform Corrosion. A special form of oxygen concentration cell corrosion or crevice corrosion occurring on metal surfaces with an organic coating system. You can recognize filiform corrosion by a worm-like trace of corrosion products beneath a paint film. Figures 2-10, Filiform Corrosion, and 2-11, Filiform Corrosion Before and After Paint Removal, illustrate this corrosion. Filiform occurs when atmospheric relative humidity is between 78 and 90 percent and the metal surface is slightly acidic. Corrosion starts at breaks in the coating system and moves underneath the coating due to diffusion of water vapor and airborne oxygen through the coating. Filiform corrosion can attack steel and aluminum surfaces. The corrosion can lead to intergranular corrosion, especially around fasteners and at seams, if filiform corrosion is not removed, treat the area, and apply a protective finish. Prevention of filiform corrosion can involve storing aircraft in an environment with a relative humidity below 70 percent, using coating systems having a low rate of diffusion for oxygen and water vapors, and by washing aircraft to remove acidic contaminants, such as airborne pollutants, from the surface.

Figure 2-10. Filiform Corrosion

Figure 2-11. Filiform Corrosion Before and After Paint Removal

2.6 Corrosion and Mechanical Factors. Mechanical factors often aggravate corrosive attack by either residual loading inside the part, or by cyclic service loads applied to the part. The extent of the attack can be influenced by environmental conditions, alloy composition, erosion by sand or rain, and mechanical wear. These factors will combine to remove surface protective films and contribute to corrosive attack of underlying metal surfaces. Corrosive attack aided by a mechanical factor usually causes the part to degenerate faster than if it is only corroding. Examples of this kind of alliance between corrosion and mechanical factors are stress-corrosion cracking, corrosion fatigue, and fretting corrosion.

2.6 Corrosion and Mechanical Factors. › 2.6.1 Stress-Corrosion Cracking.

2.6.1 Stress-Corrosion Cracking. Stress-corrosion cracking is an intergranular cracking of a metal caused by combined stress and corrosion, and Figures 2-12 through 2-14 illustrate this. Stress may come from internal or external loading. Causes of internal stresses include nonuniform deformation during cold working, unequal cooling from high temperatures, or internal structural rearrangement involving volume changes. Internal stresses result when a structure is deformed during an assembly operation, such as during pressing in bushings, shrinking a part for press fit, installing interference bolts, or installing rivets. Concealed stress is more critical than design stress because stress-corrosion is difficult to recognize before it has overcome the structure’s design safety factor. The level of stress varies from point to point within the metal, and stresses near the yield strength generally promote stress-corrosion cracking. Specific environments which cause stress-corrosion cracking of certain alloys have been identified. Salt solutions and seawater may cause stress-corrosion cracking of

high-strength, heat-treated steel and aluminum alloys. Methyl alcohol-hydrochloric acid solutions will cause stress-corrosion cracking of some titanium alloys. Magnesium alloys may stress-corrode in moist air. Stress-corrosion may be reduced by applying protective coatings, using a stress relief heat treatment, applying corrosion inhibitors, or controlling the environment. Shot peening a metal surface creates compressive stresses on the surface which help reduce stress-corrosion cracking and increase the threshold stress level.

Figure 2-12. Stress-Corrosion Cracking of 7079-T6 Fitting

Figure 2-13. Stress-Corrosion Cracking Starting at a Pit in CRES Material

Figure 2-14. Stress-Corrosion Cracking of an Extruded Section

2.6 Corrosion and Mechanical Factors. › 2.6.3 Fretting Corrosion.

2.6.2 Corrosion Fatigue. Cyclic stress and corrosion combine to form this type of stress in two stages. No metal is immune to cyclic stressing if the metal is in a corrosive environment. However, damage from corrosion fatigue is greater than damage from both cyclic stresses and corrosion. Corrosion fatigue failure occurs in two stages. During the first stage, corrosion and cyclic stress severely damage the metal by pitting and crack formation. Fracture by cyclic stressing will ultimately occur, even if the corrosive environment is completely removed. The second stage is propagation of the crack, often spreading from corrosion pits. Stress concentration effects and the physical properties of the metal primarily control the cracking. Fracture of a metal part by fatigue corrosion generally occurs at a stress level far below the fatigue limit in laboratory air, even though corrosion is relatively minor. For this reason, it is particularly important to protect all parts subject to cyclic stress, even in mildly corrosive environments.

2.6.3 Fretting Corrosion. Damage can occur at the interface of two highly loaded surfaces held immobile against each other. However, vibration may cause the surfaces to rub together resulting in an abrasive wear called fretting. This rubbing action removes any protective film on the metallic surfaces. Continued rubbing of the two surfaces prevents formation of protective oxide film and exposes fresh active metal to the atmosphere. Fretting can cause severe pitting, as shown in Figure 2-15, Fretting Corrosion and Cracking from Cyclic Loading of Lug. Prevention measures include vibration dampening, tightening joints, applying a lubricant, or installing a fretting-resistant material between the two surfaces.

Figure 2-15. Fretting Corrosion and Cracking from Cyclic Loading of Lug

2.7 Common Corrosive Agents. › 2.7.1 Acids.

2.6.4 Heat Treatment. Rigidly control heat treatment of airframe materials to maintain corrosion resistance and improve essential mechanical properties. If heat treatment of a clad aluminum alloy is too long or at too high a temperature, this may diffuse the cladding, degrade the cladding’s inherent resistance to corrosion, and reduce its protection of the core aluminum alloy. Aluminum alloys with heavy amounts of copper and zinc are highly vulnerable to intergranular corrosion attack if not quenched rapidly during heat treatment. Stainless steel alloys are susceptible to carbide sensitization when slowly cooled after welding or after high temperature heat treatment. Post-weld heat treatments are normally advisable for reduction of residual stress.

2.6.5 Hydrogen Embrittlement.

2.6.5.1 Environmentally induced failures may often be the result of hydrogen damage rather than oxidation. Atomic hydrogen is a cathodic product of many electrochemical reactions, forming during naturally occurring corrosion reactions, as well as during many plating or pickling processes. Whether hydrogen is liberated as a gas or atomic hydrogen is absorbed by the metal depends on the surface chemistry of the metal.

2.6.5.2 Atomic hydrogen, due to its small size and mass, has very high diffusivity in most metals, and penetrates most clean metal surfaces easily and migrates rapidly to favorable sites where it may remain in solution; precipitate as molecular hydrogen to form small pressurized cavities, cracks, or large blisters; or react with the base metal or with alloying elements to form hydrides.

2.6.5.3 The accumulation of hydrogen in high-strength alloys often leads to cracking, which often occurs in statically loaded components several hours or even days after applying a load or after exposure to a hydrogen source. This type of cracking is also called hydrogen stress cracking, hydrogen delayed cracking, or hydrogen-induced cracking. Similar fracture processes can occur in new and unused parts after heat treatments or machining then exposure to a hydrogen source. For this reason, processing must use well-controlled conditions to minimize the amount of hydrogen generated in processes such as pickling or electroplating.

2.7 Common Corrosive Agents. Substances that cause corrosion of metals are called corrosive agents. The most common of these agents are acids, alkalis, and salts. The atmosphere and water, the two most common media for these agents, may act as corrosive agents as well.

2.7.1 Acids. In general, moderately strong acids will severely corrode most airframe alloys. The most destructive of these corrosive agents are sulfuric acid, present in battery acid; halogen acids, such as hydrochloric, hydrofluoric, and hydrobromic acids; nitrous oxide compounds; and organic acids in human and animal wastes.

2.7.5 Water. › 2.7.5.2 The corrosive effects of fresh water vary from locality to…

2.7.2 Alkalis. Although alkalis are generally not as corrosive as acids, alkali solutions aggressively attack aluminum and magnesium alloys unless they contain a corrosion inhibitor. Washing soda; potash, of which wood ashes are an example; and lime, with cement dust as an example, are particularly corrosive to aluminum. However, ammonia, another alkali, is an exception because aluminum alloys are highly resistant to it.

2.7.3 Salts. Most salt solutions are good electrolytes and can promote corrosive attack. Some stainless steel alloys are resistant to salt solutions, but aluminum alloys, magnesium alloys, and other steels are extremely vulnerable. It is harmful to expose airframe materials to salts or salt solutions.

2.7.4 The Atmosphere. Major corrosive agents existing in atmospheric air are oxygen and airborne moisture, both in abundant supply. Corrosion often results from direct action of atmospheric oxygen and moisture on metal, and additional moisture often accelerates corrosive attack, particularly on ferrous alloys. However, the atmosphere in industrial and marine environments may also contain other corrosive gases and contaminants which are unusually corrosive.

2.7.4.1 Industrial atmospheres contain many contaminants, but most common are partially oxidized sulfur compounds. When these sulfur compounds combine with moisture, they form highly corrosive, sulfur-based acids destructive to most metals. At chemical industrial plants, other corrosive atmospheric contaminants may be present in large quantities, but such conditions are usually confined to a specific location.

2.7.4.2 Marine atmospheres contain chlorides such as salt particles or droplets of salt-saturated water. Since salt solutions are electrolytes, they corrosively attack aluminum and magnesium alloys, which are vulnerable to this type of environment.

2.7.5 Water. The corrosiveness of water depends on the dissolved minerals, organic impurities, and dissolved gasses, particularly oxygen, in the water. One characteristic of water which promotes corrosion is conductivity, or the ability to act as an electrolyte and conduct a current. Physical factors, such as water temperature and velocity, also have a direct bearing on corrosiveness.

2.7.5.1 The most corrosive of natural waters, seawater, and fresh waters are those that contain salts. Seawater is extremely corrosive due to the presence of chloride ions, but waters in harbors are often more corrosive because of industrial waste contamination combined with seawater.

2.7.5.2 The corrosive effects of fresh water vary from locality to locality due to the concentration of dissolved impurities in any particular area. Some municipal potable water supplies with chlorine and fluorides added can be quite corrosive. Commercially softened water and industrially polluted rain water are usually very corrosive.

2.8 Microorganisms. › 2.8.6 Damage resulting from microbial growth can occur when any, or a…

2.8 Microorganisms.

2.8.1 Microbial corrosive attack comes from the actions of bacteria, fungi, or molds. Microorganisms occur nearly everywhere, and bacteria and fungi cause the greatest corrosion problems.

2.8.2 Bacteria may be either aerobic, requiring oxygen to live, or anaerobic, surviving only when free oxygen is not present. Bacteria accelerate corrosion by oxidizing sulfur to produce sulfuric acid. Bacteria living adjacent to metals may promote corrosion by depleting the oxygen supply or releasing metabolic by-products oxidation of inorganic compounds such as iron, sulfur, hydrogen, or carbon monoxide. The resultant chemical reactions cause corrosion.

2.8.3 Fungi are the growths of microorganisms that feed on organic materials. While low humidity does not kill microbes, it slows their growth and may prevent corrosion damage. Ideal growth conditions for most microorganisms are: 1) temperatures between 68 °F and 104 °F, or 20 °C and 40 °C, and 2) relative humidity between 85 percent and 100 percent. Mold, bacteria, or other microbes attack some moisture-proofing coatings, especially if the coated surfaces are contaminated. This is counter to the former belief that operators could prevent fungal attack by either applying moisture-proofing coatings to nutrient materials, or by drying compartment interiors with desiccants. Microbial growth occurs at the interface of water and an aviation fuel, where the fungus feeds only on a fuel. Fungi produce organic acids, alcohols, and esters as a by-product of their growth, and these by-products provide even better growing conditions for the fungus. The fungus typically attaches itself to the bottom of a tank, looks like a brown deposit on the tank coating when the tank is dry, and may start growing again when water and fuel are present.

2.8.4 The spore form of some microorganisms can remain dormant for long periods while dry and can become active when moisture is available. When desiccants become saturated and cannot absorb moisture passing into the affected area, microorganisms can begin to grow. Dirt, dust, and other airborne contaminants are the least recognized contributors to microbial attack. Unnoticed, small amounts of airborne debris may be sufficient to promote fungal growth.

2.8.5 As a rule of thumb, fungi nutrients are only those materials derived from plants or animals. Thus, wool, cotton, rope, feathers, and leather provide sustenance for microbes, while metals and minerals do not. This rule of thumb is mainly still valid, but the increasing complexity of synthetic materials makes it difficult or impossible to determine from the name alone whether a material will support fungus. Many otherwise resistant synthetics are susceptible to fungal attack by chemicals added to change a material’s properties.

2.8.6 Damage resulting from microbial growth can occur when any, or a combination of, three basic mechanisms come into play. First, fungi are damp and have a tendency to hold moisture, which contributes to other forms of corrosion. Second, because fungi are living organisms, they need food to survive. This food is obtained from the material on which

CHAPTER 2. CORROSION THEORY › 2.10–2.99. RESERVED.

the fungi are growing. Third, these microorganisms secrete corrosive fluids that attack many materials, including some that are not fungi nutrient.

2.8.7 Remove microbial growth completely to avoid corrosion. A common practice is to remove microbial growth by hand with a firm, nonmetallic bristle brush and water. Microbial growth removal is easier if the growth is kept wet with water. Microbial growth may also be removed with steam at 100 pounds per square inch (psi) and steam temperatures not exceeding 150 °F, or 66 °C. Protective clothing should be worn when using steam for removing microbial growth.

Note: Steam at 100 psi may damage, lift, or remove some paints or sealants.

2.9 Metallic Mercury Corrosion on Aluminum Alloys. Spilled mercury on aluminum should be cleaned immediately because mercury causes corrosion attack, which is rapid in both pitting and intergranular attack and is very difficult to control. The most devastating effect of mercury spillage on aluminum alloys is the formation of an amalgam which proceeds rapidly along grain boundaries, causing liquid metal embrittlement. If the aluminum alloy part is under tension stress, this embrittlement will result in splitting with an appearance similar to severe exfoliation. X ray inspection may be an effective method of locating the small particles of spilled mercury because the dense mercury will show up readily on the x ray film.

2.10–2.99. RESERVED.

3.2 Effects of Corrosion on Metals. › 3.2.2 Steel.

CHAPTER 3. EFFECTS OF CORROSION

3.1 General. Most metals corrode, but corrosion can be minimized by using corrosion-resistant metals and finishes. The principal material in airframe structures is high-strength aluminum alloy sheet coated, or clad, with a pure aluminum coating, called Alclad, which is highly resistant to corrosive attack. However, pitting of the Alclad will occur with an accumulation of airborne salts or industrial pollutants, and an electrolyte, such as moisture. Once the Alclad surface is broken, rapid deterioration of the high-strength aluminum alloy below occurs. Other metals commonly used in airframe structures require special preventive measures to guard against corrosion, such as non-clad, high-strength aluminum alloys, steel, and magnesium alloys.

3.1.1 Aluminum alloys typically have anodize or conversion coatings, which are primed or primed and topcoated. In some later generation aircraft, operators apply an aluminum plating using the ion vapor disposition (IVD) process, then prime and possibly topcoat the surface with paint.

3.1.2 Brass and bronze require cadmium plating, zinc plating, IVD aluminum coating, or a conversion coating. Most stainless steels do not need this protective coating.

3.1.3 Magnesium alloys are highly susceptible to corrosion attack, especially where airborne salts or industrial pollutants are present, and require special chemical and electrochemical treatments and paint finishes.

3.2 Effects of Corrosion on Metals. Below is a list of the characteristics and common properties of corrosion in commonly used aircraft metals:

3.2.1 Magnesium. This is a chemically active metal used in airplane construction, highly susceptible to corrosion, and difficult to protect. When a failure in the protective coating occurs, the coating should be promptly and completely repaired to avoid serious structural damage. Magnesium corrosion is possibly easiest to detect since, even in its early stages, corrosion products occupy several times the volume of the original magnesium metal. The beginning attack appears as a lifting of the paint film and as white spots on the surface which rapidly develop into snow-like mounds or whiskers. Correction of damage involves completely removing corrosion and applying a chemical conversion coat and protective finish. Magnesium always requires protective coatings, and some magnesium parts in current aircraft have been initially protected by proprietary electrolytic processes, such as HAE and DOW 17 coatings. The HAE process can be identified by the brown or mottled gray appearance of the unpainted surface. DOW 17 coatings have a green to grayish-green color. Electrolytic coatings are thicker than those applied by immersion or brushing. Electrolytic finishes cannot be restored in the field. Take care to minimize removal and repair of these coatings.

3.2.2 Steel. Corrosion of steel is easily recognized because the corrosion product is red rust. When iron-based alloys corrode, dark corrosion products usually form first on the surface of the metal. These products are protective, but if moisture is present, this ferrous oxide coating is converted to hydrated ferric oxide, or red rust. This material will promote

3.2 Effects of Corrosion on Metals. › 3.2.6 Cadmium and Zinc.

further attack by absorbing moisture from the air. The most practical means of controlling corrosion of steel is complete removal of corrosion products by mechanical means and by maintaining the protective coating system, usually by a plating, and often combined with a paint system.

Note: Stainless steels generally do not exhibit red rust and should be assessed with the criteria in paragraph 3.2.7.

3.2.3 Aluminum. Aluminum and its alloys exhibit a wide range of corrosive attack, including uniform surface, galvanic, pitting, intergranular, exfoliation, crevice, stress, and fretting corrosion (see paragraphs 2.5 and 2.6). Where airborne salts or industrial pollutants are present, all aluminum alloys require protection. The corrosion product of aluminum is a white-to-gray powdery material which can be removed by mechanical polishing or brushing with materials softer than the metal. General surface attack of aluminum penetrates slowly but is accentuated in the presence of dissolved salts in an electrolyte. Corrosion must be addressed when present, even in small amounts. Some alloys resist general corrosion and instead corrode by pitting or intergranular attack, which can affect the structural strength without appearing widespread. However, at least three forms of attack on aluminum alloys are particularly serious:

1. Penetrating, pit-type corrosion through walls of aluminum tubing.

2. Stress-corrosion cracking of materials under sustained stress and corrosive environment.

3. Intergranular attack characteristic of certain alloys where clearly defined grain boundaries differ chemically from the metal within the grain.

3.2.4 Anodized Aluminum. Some aluminum parts are protected with an anodized coating. Aluminum oxide film on aluminum is naturally protective, and anodizing merely increases the thickness of the oxide film. When this coating is damaged in service, the coating can be partially restored by chemical surface treatment. As only partial restoration is possible, avoid unnecessary destruction of the anodized surface when performing any processing of the surface.

3.2.5 Titanium. Titanium is prone to cause severe corrosion of adjacent parts through galvanic corrosion. Titanium parts may be galvanically isolated from adjacent parts through barrier coatings or films. Frequent inspection for degradation of these barrier films and inspection for corrosion of adjacent parts is recommended. Contact with zinc and cadmium-plated parts can promote cracking of the titanium.

3.2.6 Cadmium and Zinc. Cadmium as a coating protects steel parts and provides a compatible surface when a part contacts other materials. Attack on cadmium is evidenced by a white-to-brown-to-black mottling of the surface. Zinc forms large amounts of white corrosion products. When cadmium and zinc plate show mottling and isolated voids or cracks in the coating, the plating is still performing its protective function. The cadmium plate on iron or steel is still protecting its core until actual iron rust appears.

3.2.10 Silver, Platinum, and Gold. › 3.2.10.1 When silver is plated over copper, accelerated corrosion of…

Note: Any mechanical removal of corrosion products should be limited to metal surfaces from which the cadmium has been depleted.

3.2.7 Stainless Steels. These metals are iron-base alloys containing 12 percent or more chromium and other elements, with both magnetic and nonmagnetic properties. Magnetic steels are identified by numbers in the American Iron and Steel Institute (AISI) 400 series, such as 410 or 430. These steels are less corrosion resistant than the nonmagnetic alloys, which you identify by numbers in the AISI 300 series, such as 304 or 316. The AISI 300-series steels have nickel content ranging from 6 to 22 percent, while 400-series steels have nickel content of only 2 percent. The corrosion resistance of these steels lies in their ability to form a protective oxide film on the surface. This “passive” film can be reinforced by treatment in certain chemical solutions. However, such steels will also pit when exposed to harsh corrosive environments, such as airborne salts and industrial pollutants. Stainless steels are highly susceptible to crevice/concentration cell corrosion and stress-corrosion cracking in moist, salt-laden environments and can cause galvanic corrosion of almost any other metal with which they are in contact if proper techniques of sealing and protective coating are ignored. Precipitation hardening stainless steels such as PH17-4, PH15-5, and PH13-8Mo. are now more widely used as compared to 400 series stainless. Corrosion can be prevented by keeping stainless steel clean.

3.2.8 Nickel and Chromium. These metals are protective coatings and alloying elements with iron in stainless steels. Chromium plating also provides a smooth, wear-resistant surface and reclaims worn parts. A nickel undercoat enhances corrosion resistance in a marine environment. The degree of protection is dependent upon plating thickness. Both metals form continuous oxide coatings that you can polish to a higher luster and still protect not only themselves but any underlying metal. Chromium coatings contain cracks, and corrosion originates in these separations.

3.2.9 Copper and Copper Alloys. These are generally corrosion resistant. However, the effects of minor amounts of corrosion on copper electrical components can appreciably degrade the performance of the components. The product of corrosion on copper is generally a bluish-green coating on the surface of the material. When coupled with most metals used in aircraft construction, copper is the less chemically active metal and greatly accelerates corrosion of other metals.

3.2.10 Silver, Platinum, and Gold. These metals do not corrode in the ordinary sense, although silver tarnishes as a brown-to-black film in the presence of sulfur. Gold tarnish is very thin and shows up as a darkening of reflecting surfaces.

3.2.10.1 When silver is plated over copper, accelerated corrosion of the copper through galvanic action can occur at pinholes or breaks in the silver plating. This corrosion is “red plague,” and presents as a brown-red powder deposit on the exposed copper.

3.2 Effects of Corrosion on Metals. › 3.2.11 Tin.

3.2.10.2 “Purple plague” is a brittle gold-aluminum compound formed when bonding gold to aluminum. The growth of such a compound can cause failure in microelectronic interconnection bonds.

3.2.11 Tin. This material is common on radio frequency (RF) shields, filters, crystal covers, and automatic switching devices. Tin has the best combination of solderability and corrosion resistance of any metallic coating.

Table 3-1. Corrosion of Metals

ALLOY TYPE OF ATTACK TO WHICH

ALLOY IS SUSCEPTIBLE

APPEARANCE OF CORROSION PRODUCT

Magnesium Highly susceptible to pitting White, powdery, snow-like mounds and white spots on surface

Low Alloy Steel (4000–8000 series)

Surface oxidation and pitting, surface, and intergranular

Reddish-brown oxide (rust)

Aluminum Surface pitting, intergranular, exfoliation stress­corrosion and fatigue cracking, and fretting

White-to-gray powder

Titanium Highly corrosion resistant; extended or repeated contact with chlorinated solvents may result in degradation of the metal’s structural properties at high temperature

No visible corrosion products at low temperature. Colored surface oxides develop above 700 °F, or 370 °C

Cadmium Uniform surface corrosion; used as sacrificial plating to protect steel

From white powdery deposit to brown or black mottling of the surface

Stainless Steels (300-400 series)

Crevice corrosion; some pitting in marine environments; corrosion cracking; intergranular corrosion (300 series); surface corrosion (400 series)

Rough surface; sometimes a uniform red, brown, stain

Nickel Alloy Generally corrosion-resistant; exposure to very high temperatures in air can lead to corrosion product formation on the surface of parts made from nickel; exposure to stagnant seawater can lead to surface pitting due to crevice/concentration cell corrosion

Green powdery deposit on the surface

Nickel-Based (Inconel, Monel)

Generally has good corrosion resistant qualities; susceptible to pitting in sea water

Green powdery deposit

Copper-Based Brass, Bronze

Surface and intergranular corrosion Blue or blue-green powdery deposit

Chromium (Plate) Pitting; promotes rusting of steel where pits occur in plating

No visible corrosion products; blistering of plating due to rusting and lifting

ALLOY TYPE OF ATTACK TO WHICH

ALLOY IS SUSCEPTIBLE

APPEARANCE OF CORROSION PRODUCT

Silver Will tarnish in the presence of sulfur Brown-to-black film

CHAPTER 3. EFFECTS OF CORROSION › 3.3–3.99. RESERVED.

Gold Highly corrosion resistant Deposits cause darkening of reflective surfaces

3.3–3.99. RESERVED.

CHAPTER 4. CORROSION-PRONE AREAS AND PREVENTIVE MAINTENANCE

4.1 General. This chapter lists corrosion problem areas common to most aircraft. Be aware to clean, inspect, and treat corrosion-prone areas more frequently. The list is not intended for a specific aircraft, but it can be used to set up a maintenance inspection program. This chapter also includes factors in corrosion control and preventive maintenance.

CHAPTER 4. CORROSION-PRONE AREAS AND PREVENTIVE MAINTENANCE › 4.3 Battery Compartments and Battery Vent Openings.

4.2 Exhaust Trail Areas. Both jet and reciprocating engine exhaust gas deposits are very corrosive. Inspection and maintenance of exhaust trail areas should include attention to areas indicated in Figure 4-1, Exhaust Trail Area Corrosion Control Points, and inspection should include removal of fairings and access plates in the exhaust gas path.

4.2.1 Gaps, seams, hinges, and fairings are areas where exhaust trail deposits may be trapped and normal cleaning methods cannot reach these areas.

4.2.2 Exhaust deposit buildup on the upper and lower wing, aft fuselage, and in the horizontal tail surfaces will be considerably slower and sometimes completely absent on certain aircraft models.

Figure 4-1. Exhaust Trail Area Corrosion Control Points

4.3 Battery Compartments and Battery Vent Openings. In spite of protective paint systems and extensive sealing and venting, battery compartments continue to be corrosion problem areas. Fumes from overheated battery electrolyte are difficult to contain and can spread to internal structures where unprotected surfaces can come under corrosive attack. For lead-acid batteries, frequent cleaning and neutralization of acid deposits with sodium bicarbonate solution will minimize corrosion. If the battery

CHAPTER 4. CORROSION-PRONE AREAS AND PREVENTIVE MAINTENANCE › 4.6 Wheel Wells and Landing Gear.

installation includes external vent openings on the aircraft skin, these areas should be included in inspection and maintenance procedures. If aircraft have batteries with electrolytes of either sulfuric acid or potassium hydroxide, electrolyte leakage will cause corrosion. Consult applicable maintenance manuals to determine the battery type installed and recommended maintenance practices. Clean nickel cadmium compartments with ammonia or boric acid solution, dry thoroughly, then paint with an alkali-resistant varnish.

4.4 Lavatories, Buffets, Galleys, Doorways, and Cockpit Floorboards. These areas, particularly deck areas behind lavatories, sinks, and ranges, are potential trouble areas where spilled food and waste products may collect. Even though some contaminants are not corrosive, they will attract and retain moisture, and promote corrosive attack. Pay particular attention to bilge areas and aircraft structure located under galleys and lavatories. Clean these areas frequently and maintain protective sealant and paint finishes.

Figure 4-2. Typical Damage to Floor Around Lavatories, Buffets, and Galleys

4.5 Bilge Areas. On all aircraft, the bilge area is a common trouble area. The bilge is a natural sump or collection point for waste hydraulic fluids, water, dirt, loose fasteners, drill chips, and other debris. Residual oil quite often masks small quantities of water which settle to the bottom and set up a hidden potential corrosion cell. Except for water displacing corrosion-preventing compounds, keeping bilge areas free of extraneous material, including water and oil, will insure the best protection against corrosion. A good vacuum cleaner and clean wiping cloths are handy tools to clean such areas.

4.6 Wheel Wells and Landing Gear. The wheel well area probably receives more punishment than any other area of the aircraft. It is exposed to mud, water, salt, gravel,

CHAPTER 4. CORROSION-PRONE AREAS AND PREVENTIVE MAINTENANCE › 4.6.2 During inspection of this area, pay particular attention to these…

and other flying debris from runways during flight operations. See Figure 4-3, Landing Gear and Wheel Corrosion Points.

4.6.1 Aircraft wheels and wheel well areas should receive frequent cleaning, lubrication, and paint touch-up. Because of many complicated shapes, assemblies, and fittings in the area, complete coverage with a protective paint film is difficult, and preservative coatings tend to mask trouble rather than prevent it. Do not use preservative coatings on landing gear wheels because of the heat generated from braking.

4.6.2 During inspection of this area, pay particular attention to these trouble areas:

• Aluminum and high-strength steel.

• Exposed surfaces of struts, oleos, arms, links, and attaching hardware, such as bolts or pins.

• Axle interiors.

• Exposed position indicator switches and other electrical equipment.

• Crevices between stiffeners, ribs, and lower skin surfaces, typical water and debris traps.

• Magnesium wheels, particularly around bolt heads, lugs, and wheel web areas.

• Exposed rigid tubing, especially at “B” nuts and ferrules under clamps and tubing identification tapes.

Figure 4-3. Landing Gear and Wheel Corrosion Points

4.7 External Skin Areas. External aircraft surfaces are ordinarily covered with protective finishes, and operators can also apply paint coatings. Affected external aircraft surfaces are readily visible or available for inspection and maintenance. Much emphasis has been given to these areas in the past, and maintenance procedures are well established. Even here, certain configurations or combinations of materials become troublesome and require special attention to avoid serious corrosion difficulties. Some common trouble areas are listed below, other than those attributed to engine exhaust deposits:

4.7 External Skin Areas. › 4.7.2 Faying Surfaces and Crevices.

4.7.1 Steel, Titanium, Corrosion Resistant Steel (CRES), and Nickel Alloy Fasteners. Fasteners, and areas around these fasteners, are trouble areas. These areas are subject to high operational loads, moisture intrusion, and dissimilar metal skin corrosion. See Figure 4-4, Intergranular Corrosion of 7075-T6 Aluminum Adjacent to Steel Fastener.

Figure 4-4. Intergranular Corrosion of 7075-T6 Aluminum Adjacent to Steel Fastener

4.7.2 Faying Surfaces and Crevices. Similar to corrosion around fasteners, corrosion in faying surfaces, seams, and joints results from intrusion of moisture and other corrosive agents. The effect of this type of corrosion is usually detectable by bulging of the skin surface.

4.7.4 Spot-Welded Skins. › 4.7.4.1 Spot-welded assemblies are particularly corrosion prone, and…

Figure 4-5. Crack and Skin Bulging Caused by Corrosion

4.7.3 Magnesium Skins. Properly surface-treated, insulated, and painted magnesium skin surfaces give relatively little corrosion-related trouble if the original surface is maintained. However, trimming, drilling, and riveting destroy some of the original surface treatment, which may not be completely restored by touch-up procedures.

4.7.3.1 Some aircraft have steel fasteners installed through a magnesium skin, with only protective finishes under the fastener heads and fillet sealant or tape over the surface for insulation. Paint coatings are inherently thin at abrupt changes in contour, such as at trimmed edges. With magnesium’s sensitivity to moisture, these conditions add up to a potential corrosion problem whenever magnesium is used.

4.7.3.2 Corrosion inspections should include all magnesium skin surfaces and magnesium fittings or structural components, with special attention to edges, areas around skin edges and fasteners, and cracked, chipped, or missing paint.

4.7.4 Spot-Welded Skins. Corrosion of this type is chiefly the result of the entrance and entrapment of moisture or other corrosive agents between layers of metal. See Figure 4-6, Spot-Welded Skin Corrosion.

4.7.4.1 Spot-welded assemblies are particularly corrosion prone, and corrosive attack causes skin buckling or spot-weld bulging and fracture. This type of corrosion is evidenced by corrosion products appearing at crevices through which the corrosive agents enter. Some corrosion may originate from fabricating processes, but its progress to the point of skin bulging or spot-weld fracture is the direct result of moisture or other corrosive agents moving through open

4.7 External Skin Areas. › 4.7.5 Piano-Type Hinges.

gaps or seams. Weld-through sealing materials should minimize this problem, but many in-service aircraft have unsealed spot-weld skin.

4.7.4.2 Corrosion may appear at either external or internal faying surfaces, but is usually more prevalent on external areas. More advanced corrosive attack causes skin buckling and eventual spot-weld fracture. Detect skin buckling in this early stage by sighting or feeling along spot-welded seams or by using a straight edge to show variations along the skin.

4.7.4.3 To prevent this condition, keep potential moisture entry points (such as gaps, seams, and holes created by broken welds) filled with a noncorrosive sealant.

Figure 4-6. Spot-Welded Skin Corrosion

4.7.5 Piano-Type Hinges. These are prime spots for corrosion due to dissimilar metal contact between the steel pin and aluminum hinge tangs. These hinges are also natural traps for dirt, salt, and moisture. Hinges tend to corrode and freeze in the closed position between inspections where they are part of access doors or plate assembly and actuated only when opened during an inspection. When the hinge is inspected, lubricate it and work it through several cycles to enhance lubricant penetration. See Figures 4-7, Hinge Corrosion Points, and 4-8, Hinge Failure Caused by Corrosion.

Figure 4-7. Hinge Corrosion Points

Figure 4-8. Hinge Failure Caused by Corrosion

CHAPTER 4. CORROSION-PRONE AREAS AND PREVENTIVE MAINTENANCE › 4.9 Engine Frontal Areas and Cooling Air Vents.

4.7.6 Heavy or Tapered Aluminum Alloy Skin Surfaces. Heavy or thick sections of most heat-treated aluminum alloys are susceptible to pitting or intergranular corrosion and exfoliation of the metal. When inspecting external skin surfaces, especially around countersunk fastener heads, look for white or gray powder deposits or metal exfoliation. This usually first appears as small, raised areas or bumps under paint film.

4.7.6.1 Treatment of this corrosive attack includes removal of all corrosion products. An example of this product removal is exfoliated metal, which is blended and polished within the limits set by the aircraft manufacturer. If corrosion products remain after reaching limits set by the aircraft manufacturer, contact the aircraft manufacturer for authorized limits. The treatment is not complete until protective surface finishes are fully restored.

4.7.6.2 Protect reworked areas with a chemical conversion coating, sealant primer, and topcoat, if applicable. Watch reworked areas for any indications of renewed corrosive activity.

4.7.7 Organic Composites. Organic composites used in aircraft can cause different corrosion problems than all-metal structures. Composites such as graphite/epoxy act as a very noble, or cathodic, material, creating the electrical potential for galvanic corrosion. The galvanic corrosion potential, coupled with different attachment methods, such as adhesive bonding, stepped structures, or locking mechanical fasteners, leads to multicomponent galvanic couples aggravated by high humidity and saltwater environments. Applying aircraft sealants over dissimilar metal/composite junctions will prevent galvanic corrosion if moisture is completely displaced from the junction. Since moisture displacement is virtually impossible during extended flight operations, the most effective method of eliminating the voltage potential is to provide a nonconductive layer between the composite and dissimilar metal surfaces, such as a fiberglass/epoxy, sealant, or a combination or the two. Application of sealants over dissimilar metal/composite junctions may mask corrosion if the seal is compromised.

4.8 Water Entrapment Areas. Corrosion will result from entrapment of moisture. Except for sandwich structures, design specifications usually require that the aircraft have low-point drains in all areas where moisture and other fluids can collect. In many cases, these drains are ineffective either because of location or because they are plugged by sealants, extraneous fasteners, dirt, grease, and debris. Potential entrapment areas are not a problem when properly located drains are functioning and the aircraft has a normal ground attitude and is resting on its landing gear. Plugging a single drain hole or altering the level of the aircraft can result in a corrosion problem if water becomes entrapped in one of these “bathtub” areas, and we recommend a daily inspection of low-point drains.

4.9 Engine Frontal Areas and Cooling Air Vents. Constant abrasion by airborne dirt and dust, bits of gravel from runways, and rain all tend to remove protective surfaces from engine frontal areas and cooling air vents. Radiator cooler cores or reciprocating engine cylinder fins, designed for heat dissipation, may not be painted. Engine accessory mounting bases usually have small areas of unpainted magnesium or aluminum on machined mounting surfaces. With moist and salt or industrial pollutant-laden air

constantly flowing over these surfaces, they are prime sources of corrosive attack. Inspection of such areas should include all sections in the cooling air path, with special attention to obstructions and crevices where salt deposits may build up during marine operations. See Figures 4-9, Reciprocating Engine Frontal Area Corrosion, and 4-10, Jet Engine Frontal Area Corrosion Points.

Note: When applicable, refer to the engine manufacturer’s specific instructions for further guidance.

Figure 4-9. Reciprocating Engine Frontal Area Corrosion

4.10 Electronic Package Compartments. › 4.10.2 Only qualified personnel familiar with the function of the unit…

Figure 4-10. Jet Engine Frontal Area Corrosion Points

4.10 Electronic Package Compartments. These areas are cooled by ram air or compressor bleed air and are subject to the same conditions as engine and accessory cooling vents and engine frontal areas. While the degree of exposure is less because of a lower volume of air passing through the compartment and special design features preventing water formation in enclosed spaces, this is still a trouble area needing special attention.

4.10.1 As circuit breakers, contact points, and switches are extremely sensitive to moisture and corrosive attack, inspect for these conditions as thoroughly as the design permits. If design features hinder examination of these items while installed, inspect the items if components are removed for other reasons.

4.10.2 Only qualified personnel familiar with the function of the unit involved should perform or direct the treatment of corrosion in electrical and electronic components, as conventional corrosion treatment may damage some units.

4.11 Miscellaneous Trouble Areas. › 4.11.1 Examine and replace all flexible hose assemblies with chafing,…

4.10.3 Most corrosion on avionic equipment is similar to basic airframe structure corrosion, but there is a difference: minute amounts of corrosion in avionic equipment can cause serious degradation or complete failure, while similar corrosion on larger structures would go unnoticed.

4.10.4 Smog, smoke, soot, and other airborne contaminants are extremely corrosive to exposed avionic equipment. Many fumes and vapors emitted from factories or industrial complexes are highly acidic and greatly accelerate corrosion. An example is the corrosive effect of ozone, a product of welding machines and large electrical motors. Complete degradation of rubber seals and damage to delicate components have occurred in equipment stored near ozone-producing equipment. Avionic shops and storage areas should have a filtered air conditioning system to help remove ozone from the enclosed shop or storage area.

4.10.5 Another man-made atmosphere is the aircraft environmental control system. These systems direct cooling air to the equipment and may include a filter system that extracts moisture or contaminants from air entering the equipment. Always replace or clean filters, or eliminate leaky environmental seals, to prevent buildup of moisture or contaminants that could cause a corrosive atmosphere inside the equipment.

4.10.6 The control of corrosion in avionic systems is similar to that in airframes, with modifications. Factors affecting corrosion control in avionic equipment include:

• Less durable protection systems;

• Small amounts of corrosion can make equipment inoperative;

• Dissimilar metals are often in electrical contact;

• Stray currents can cause corrosion;

• Active metals and dissimilar metals in contact are often unprotected;

• Closed boxes can produce condensation during normal temperature changes during flight;

• Avionic systems have many areas to trap moisture;

• Hidden corrosion is difficult to detect in many avionic systems;

• Many materials in avionic systems are subject to attack by bacteria and fungi; and

• Organic materials, when overheated or improperly or incompletely cured, can produce vapors corrosive to electronic components and damaging to coatings and insulators.

4.11 Miscellaneous Trouble Areas. Additional trouble areas exist, some of which are covered by manufacturer publications. Below is a list of common trouble areas:

4.11.1 Examine and replace all flexible hose assemblies with chafing, weather checking, hardening, discoloration, evidence of fungus, and torn weather protective coatings or sleeves.

4.11.5 Electrical connectors or components may be potted with a sealing… › 4.11.5.3 When electrical components cannot be sealed, these components…

4.11.2 Trimmed edges of sandwich panels and drilled holes should have some type of corrosion protection. We recommend a brush treatment with an inhibitor solution or applying a sealant along the edge, or both. With a sealant, fill gaps or cavities where moisture, dirt, or other foreign material can settle. Adjacent structures, not the sandwich, should have sufficient drainage to prevent moisture accumulation. Seal damage or punctures in panels as soon as possible to prevent additional moisture entry, even if permanent repair must be delayed.

4.11.3 Control cables may present a corrosion problem whether of carbon steel or stainless steel construction. Bare spots in the preservative coating are a main contributing factor in cable corrosion. Determine cable condition by cleaning the cable assembly, inspecting for corrosion, and applying an approved preservative if no corrosion is found. If external corrosion is found, relieve tension on the cable and check internal strands for corrosion. Cables with corrosion on internal strands should be replaced. Pay particular attention to sections passing through fairleads, around sheaves, and grooved bell-crank arms. External corrosion should be removed by a clean, dry, coarse rag or fiber brush. After complete corrosion removal, apply a preservative.

4.11.4 Topcoating materials in integral fuel cells, such as Buna-N, polyurethane, or epoxy, repel fuel but can absorb moisture through the topcoating materials and sometimes cause pitting or intergranular corrosion on aircraft structural parts. We have also found that microorganisms which live in water entrained by fuel, particularly jet propellant fuel types, feed on fuel hydrocarbon and hydrocarbon-type elastomeric coating materials. Excreted organic acids and dead microorganisms act as a gelatinous acidified sponge which can deteriorate integral tank coatings and corrode the aircraft structure. Minimize microbial corrosion by preventing as much water contamination of the fuel as possible with well-managed storage facilities, adequate fuel filtration, and drainage of water contamination from integral fuel cells. This drainage keeps the water moving and reduces development of microorganism colonies. Reduce microorganic activity by using a biocide additive such as “Biobor JF” or equivalent. Use manufacturer instructions to determine solution strength and application frequency.

4.11.5 Electrical connectors or components may be potted with a sealing compound for improved reliability, and to prevent moisture entrance into connectors where wires are attached to pins.

4.11.5.1 Use rubber O-rings to keep moisture out of the mating area of pin connections and prevent loss of pressurization in compartments containing bulkhead connectors.

4.11.5.2 Moisture intrusion into electrical connectors can cause corrosion and an electrical failure. Disconnect and disassemble suspected plugs, clean with a solvent, and inspect for corrosion.

4.11.5.3 When electrical components cannot be sealed, these components can have moisture intrusion and internal corrosion.

4.11 Miscellaneous Trouble Areas. › 4.11.8 Flap and slat recesses and equipment installed in these areas,…

4.11.6 Severe corrosion damage to rear pressure bulkheads below the floor may occur as a result of contamination by fluids. Inspection for rear bulkhead corrosion may require extensive disassembly of components and fixtures to enable a thorough visual inspection. When inspection access holes are available, inspection by fiber optics is useful. Other nondestructive inspection (NDI) methods, such as x ray, ultrasonic, and eddy current, are also available. However, these inspection techniques require specially trained personnel, NDI comparison standards, and suitable access. Regular inspections of the rear pressure bulkhead, both front and rear faces, below the floor level should prevent serious corrosion buildup between the bulkhead and periphery doubler at the floor level. Such corrosion could weaken the bulkhead skin and lead to sudden cabin pressure loss.

4.11.7 Some older aircraft develop delaminations in cold-bonded joints. Corrosion between the delaminated surfaces stems from moisture intrusion along edges of mating parts or around fasteners securing mating parts together. Localized bulging of a skin or internal structural components, usually around the fasteners, is the first indication of a corrosion problem (see Figure 4-11, Spar Chord Lifting Caused by Corrosion Products). Skin cracks or dished or missing fastener heads may also indicate severe corrosion in bonded joints. Corrosion occurring between skins, doublers, and stringers or frames will produce local bulging or pulled rivets (see Figure 4-12, Skin Bulging Around Fasteners). Corrosion that occurs between the skins and doublers or tear straps away from a backup structure, such as stringer or frame, will not produce local bulging. An external low frequency eddy current inspection should determine the extent of corrosion in the skin. Open lap joints with wedges to determine the full extent of corrosion damage (see Figures 4-13, Opening of a Corroded Lap Joint for Repair, and 4-14, Close-Up View of a Corroded Lap Joint). Internal visual inspection should detect delaminated doublers or tear straps. Apply a penetrating water displacement corrosion inhibitor to faying surfaces after corrosion removal and repair.

4.11.8 Flap and slat recesses and equipment installed in these areas, normally closed, may corrode unnoticed without special inspections.

Figure 4-11. Spar Chord Lifting Caused by Corrosion Products

Figure 4-12. Skin Bulging Around Fasteners

Figure 4-13. Opening of a Corroded Lap Joint for Repair

Figure 4-14. Close-Up View of a Corroded Lap Joint

4.12.2 Corrosion Control in Design. › 4.12.2.3 The use of corrosion-resistant alloys is not a cure-all for…

4.12 Factors in Corrosion Control.

4.12.1 Corrosion Factors. The severity, cause, and type of corrosion depend on many factors, including a part’s size or thickness, the material, heat treatment of the material, protective finishes, environmental conditions, preventive measures, and design.

4.12.1.1 Thick structural sections are generally more susceptible to corrosive attack because of variations in composition, particularly if sections are heat-treated during fabrication. When large sections are machined or chemically milled after heat treatment, corrosion characteristics of thinner sections may differ from thicker areas. Section size adheres to structural requirements and cannot be changed to control corrosion. From a maintenance standpoint, the correct approach is to recognize the need to ensure the integrity and strength of major structural parts and maintaining permanent protection over such areas at all times.

4.12.1.2 In-service stresses and field repairs may affect rates and types of corrosion. Aircraft structures under high cyclic stresses, such as helicopter main rotors, are particularly subject to stress-corrosion cracking. Areas next to weld-repaired items often have corrosion due to insufficient weld flux removal or buildup of a magnetic field. Closely inspect these areas for signs of corrosion and properly treat when found.

4.12.2 Corrosion Control in Design. Since corrosion is the deterioration of metal resulting from a reaction between a metal and its environment, some form of corrosion control or means to minimize corrosion should become part of an aircraft’s design phase before the aircraft enters operational service. The corrosion issues discussed in this AC provide information to reduce the rate of corrosive attack by corrosion control measures introduced early in design.

4.12.2.1 The nature of a material is a fundamental factor in corrosion. High-strength, heat-treatable aluminum and magnesium alloys are very susceptible to corrosion, while titanium and some stainless steel alloys are less susceptible in atmospheric environments. The aircraft manufacturer selects material for the aircraft based on material strength, weight, and cost, while corrosion resistance is often a secondary consideration. Corrosion control should be included in an aircraft’s preliminary design phase as early as possible.

4.12.2.2 More corrosion-resistant materials in any design normally involves additional weight to achieve the required strength. Weight consideration is a major factor in the construction of airframes, and the primary means of preventing corrosion is through protective coatings and proper maintenance procedures.

4.12.2.3 The use of corrosion-resistant alloys is not a cure-all for corrosion prevention. A common mistake is to replace a corroded part with a corrosion-resistant alloy; sometimes the corrosion then shifts to another part and increases in severity.

4.12.2 Corrosion Control in Design. › 4.12.2.5 Galvanic corrosion results from dissimilar metals in contact,…

4.12.2.4 Protection against corrosion is minimized if the protected material is intrinsically resistant to corrosion. Aluminum copper alloys (2000 series) are known to have better stress-corrosion resistance and better fatigue strength properties than aluminum zinc alloys (7000 series), so aircraft designers use them more often as the primary structural materials.

4.12.2.5 Galvanic corrosion results from dissimilar metals in contact, and the galvanic series of metals and alloys (see Table 4-1, Galvanic Series of Metals and Alloys) is a factor to consider in aircraft repair. The further apart the potential voltages of the metals listed in Table 4-1 are, the greater the tendency for galvanic corrosion. The metals in Table 4-2, Grouping of Metals and Alloys, have small differences in electrical potential, so they are relatively safe to use in contact with one another. However, the coupling of metals from different groups will result in corrosion of the group having a lower potential voltage. The electrode potentials as given in Table 4-1 are valid for pure materials at standard lab conditions. However, in-service conditions are different and potential voltages may shift to either side, positive or negative, as do alloying elements. Although this does not affect the general ranking, it can significantly affect the potential differences relevant for corrosion prevention and, in few cases, this may even invert ranking of two metals.

Table 4-1. Galvanic Series of Metals and Alloys

Electrode Potential of Various Metals and Alloys (a)

Metal or Alloy (b) PH stainless steels Potential, volts 0.025

0.1 N calomel scale (c)

Magnesium -1.73

Zinc -1.10

7072, Alclad 3003, Alclad 6061, Alclad 7075 -0.96

5056, 7079-T6, 5456, 5083, 214, 218 -0.87

5052, 5652, 5086, 1099 -0.85

3004, B214, 1185, 1060, 1260, 5050 -0.84

1100, 3003, 615, 6053, 6061-T6, 6062-T6, 6063, 6363, Alclad 2014, Alclad 2024

-0.83

Cadmium -0.82

7075-T6, 356-T6, 360 -0.81

2024-T81, 6061-T4, 6062-T4 -0.80

355-T6 -0.79

2014-T6, 113, 750-T5 -0.78

2014-T4, 2017-T4, 2024-T3, and T4 -0.68 to -0.70 (d)

Mild steel -0.58

Lead -0.55

Tin -0.49

Copper -0.20

Bismuth -0.18

Stainless steel (series 300, type 430) -0.09

Silver -0.08

Nickel -0.07

Chromium -0.49 to +0.018

(a) Data from Alcoa Research Laboratories.

(b) The potential of all tempers is the same unless temper is designated.

(c) Measured in an aqueous solution of 53g of sodium chloride + 3g hydrogen peroxide per liter at 25 degree c.

(d) The potential varies with quenching rate.

4.12 Factors in Corrosion Control. › 4.12.5 Heat Treatment.

Table 4-2. Grouping of Metals and Alloys

GROUP I Magnesium and Magnesium Alloys.

GROUP II Aluminum, Aluminum Alloys, Zinc, Cadmium, and Cadmium-Titanium Plate.

GROUP III Iron, Steels Except Stainless Steels; Lead, Tin, and their Alloys.

GROUP IV Copper, Brass, Bronze, Copper-Beryllium, Copper-Nickel Chromium, Nickel, Nickel Base Alloys, Cobalt Base Alloys, Carbon Graphite, Stainless Steels, Titanium, and Titanium Alloys.

NOTE: 1. Metals listed in the same group are considered similar to one another.

2. Metals listed in different groups are considered dissimilar to one another.

4.12.3 Protective Finishes. Base material with a protective finish is protected from corrosion and other forms of deterioration. These finishes have two categories: sacrificial and non-sacrificial. Sacrificial coatings include cadmium, zinc, and aluminum. Non-sacrificial coatings include hard plating, such as chromium and nickel, chemical conversion coatings, sealant, primers, and topcoat.

4.12.4 Geographical Location and Environment. This factor concerns systems exposed to marine atmospheres, moisture, acid rain, tropical temperature conditions, industrial chemicals, and soils and dust in the atmosphere. Whenever possible, limit the requirement for operation of aircraft in adverse environments.

4.12.4.1 Moisture is present in the air as a gas, also called water vapor, or as finely divided droplets of liquid, as in mist or fog, and often contains contaminants such as chlorides, sulfates, and nitrates, which increase its corrosive effects. Condensed moisture which evaporates will leave contaminants behind; become trapped in close fitting, wettable joints, such as faying surfaces; and collect along poor bond lines by capillary action.

4.12.4.2 Salt particles, when dissolved in water, form strong electrolytes. Normal sea winds carry dissolved salt which makes coastal environments highly corrosive.

4.12.4.3 Industrial pollutants, such as carbon, nitrates, ozone, sulfur dioxide, and sulfates, contribute to the deterioration of nonmetallic materials and can cause severe corrosion of metals.

4.12.4.4 Warm, moist air normally found in tropical climates accelerates corrosion while cold, dry air normally found in arctic climates reduces corrosion.

4.12.5 Heat Treatment. Proper heat treatment of materials is a vital factor in maximizing resistance to corrosion.

4.13.1 Prevention. › 4.13.1.10 Minimizing aircraft exposure to adverse environments, such as…

4.13 Preventive Maintenance.

4.13.1 Prevention. Corrosion prevention of aircraft structure depends on a comprehensive corrosion prevention and control plan, implemented from the start of operation of an aircraft, which includes:

4.13.1.1 Adequately trained personnel in:

• Recognition of corrosion-inducing conditions;

• Corrosion identification techniques;

• Corrosion detection, cleaning, and treating; and

• Lubrication and preservation of aircraft structure and components.

4.13.1.2 Scheduled inspection for corrosion.

4.13.1.3 Periodic, thorough cleaning, inspection, lubrication, and preservation. See Figures 4-15 through 4-20. Suggested intervals based on operating environment:

• Mild zones: every 90 calendar-days;

• Moderate zones: every 45 calendar-days; and

• Severe zones: every 15 calendar-days.

4.13.1.4 Prompt corrosion treatment after detection.

4.13.1.5 Accurate recordkeeping and reporting of material or design deficiencies to the manufacturer and the FAA.

4.13.1.6 Use of appropriate materials, equipment, and technical publications.

4.13.1.7 Maintenance of basic finish systems.

4.13.1.8 Keeping drain holes and passages open and functional. Sealants, leveling compounds, miscellaneous debris, or corrosion inhibitors should not block drain paths. See Figure 4-21, Blocked Drain Passages Resulted in Accumulation of Corrosion Contaminates and Moisture.

4.13.1.9 Replacing deteriorated or damaged gaskets and sealants, using noncorrosive type sealants, to avoid water intrusion and entrapment which leads to corrosion.

4.13.1.10 Minimizing aircraft exposure to adverse environments, such as hangar storage away from salt spray.

Figure 4-15. North America Corrosion Severity Map

Figure 4-16. South America Corrosion Severity Map

Figure 4-17. Africa Corrosion Severity Map

Figure 4-18. South Pacific Corrosion Severity Map

Figure 4-19. Asia Corrosion Severity Map

Figure 4-20. Europe and Asia Minor Corrosion Severity Map

4.13.2 Cleaning Compounds for Metals. › 4.13.2.3 A high-gloss spot cleaner conforming to MIL-SPEC MIL-C-85570,…

Figure 4-21. Blocked Drain Passages Resulted in Accumulation of Corrosion Contaminates

and Moisture

4.13.2 Cleaning Compounds for Metals.

Note: More is not always better, and mixing more cleaning compound increases the pH of a solution, which can do more harm than good. Always mix a cleaning compound using manufacturer recommendations.

4.13.2.1 Cleaning compounds work by dissolving soluble soils, emulsifying oily soils, and suspending solid soils. There are several cleaning compounds, and each cleans a surface using one or more of the below mechanisms.

4.13.2.2 Highly alkaline cleaning compounds (with a pH greater than 10) are not recommended. However, moderately alkaline cleaners (with a pH between 7.5 and 10) conforming to Military Specification (MIL-SPEC) MIL-C-85570, Cleaning Compounds, Aircraft, Exterior, Types I and II, are recommended. Both types contain detergents, foaming agents, and solvents, and work the same as a detergent solution.

4.13.2.3 A high-gloss spot cleaner conforming to MIL-SPEC MIL-C-85570, Type III, is recommended for cleaning exhaust track areas of high-gloss paint systems. This material contains solvents, detergents, and suspended abrasive matter to remove soil by wearing away the surface that holds it.

4.13.2 Cleaning Compounds for Metals. › 4.13.2.8 Miscellaneous cleaning agents include:

4.13.2.4 Thixotropic, or viscous, cleaner conforming to MIL-SPEC MIL-C-85570, Type V is recommended for cleaning wheel wells and replacement of some solvent cleaning where water rinsing can be used. This cleaner contains solvents, detergents, and some thickening agents. When applied undiluted to an oily or greasy surface, the cleaner clings long enough to emulsify the soil, usually about 5 to 15 minutes, then can be rinsed away with fresh water.

Note: Solvents for cleaning operations is becoming more and more limited due to environmental regulations. Determine local requirements for waste disposal.

4.13.2.5 Solvent emulsion cleaners conforming to MIL-SPECs MIL-C-43616, Cleaning Compounds, Aircraft Surface, and MIL-C-85704, Cleaning Compound, Turbine Engine Gas Path, become emulsions when diluted. The solvent in the cleaner softens oily soils so that they can be emulsified by the detergent and rinsed away.

4.13.2.6 Detergent solution cleaners conforming to MIL-SPEC MIL-D-16791, Detergents, General Purpose (Liquid, Nonionic), dissolve in water and clean by dissolving soluble salts, emulsifying low-viscosity oils, and suspending easily removed dirt and dust. They are not very effective on grease, but are excellent cleaners for interior lightly soiled areas, plastics, and instrument glass covers.

4.13.2.7 Cleaning solvents dissolve oily and greasy soils so that they can be easily wiped away or absorbed on a cloth. Solvents differ significantly in cleaning ability, toxicity, evaporation rate, effect on paint, and flammability. Cleaning solvents are best for localized spot application only. A dry cleaning solvent conforming to MIL-SPEC MIL-PRF-680, Performance Specification: Degreasing Solvent, Type II, is the most common cleaning solvent used on aircraft, due to its low toxicity, minimal effect on paint, and relative safety. Other solvents, such as alcohols, ketones, chlorinated solvents, and naphtha, are specialized materials and have restricted use. Refer to manufacturer maintenance and cleaning procedures for specific applications.

4.13.2.8 Miscellaneous cleaning agents include:

• Plastic polish, which contains mild abrasive matter to polish out scratches in canopy materials;

• Alkaline chemicals used to neutralize specific acidic soils;

• Sodium bicarbonate for electrolyte spills from sulfuric acid batteries; and

• Monobasic sodium phosphate and boric acid for electrolyte spills from nickel-cadmium batteries.

4.13.2.9 Steam cleaning is not recommended for general use on aircraft. It erodes paint, crazes plastic, debonds adhesives, damages electrical insulation, and drives lubrication out of bearings.

4.13 Preventive Maintenance. › 4.13.4 Preservation.

4.13.3 Cleaning Procedures.

4.13.3.1 The following cleaning procedures are recommended:

• Remove/disconnect all electrical power;

• Ground aircraft;

• Aircraft wash personnel should wear protective gear, such as gloves, goggles, or aprons;

• Protect against water/cleaning compound intrusion, such as at closed doors, openings, cover vents, pitot static openings, or cover wheels. Precautions should be taken to ensure these protections are removed after cleaning;

• Accomplish pre-wash lubrication. Lubricate per applicable maintenance manual;

• Mix cleaning solution per manufacturer recommendation;

• Use spray, not a stream, of water during aircraft wash;

• Do not use abrasive cleaning pads; and

• Rinse aircraft with fresh water to remove all cleaning compounds.

4.13.3.2 The following post-cleaning procedures are recommended:

• Remove all covers, plugs, and masking materials;

• Inspect and clear all drain holes;

• Inspect and open all known water trap areas for water accumulation and proper drainage;

• Lubricate aircraft per applicable maintenance manual; and

• Apply operational preservation.

4.13.4 Preservation. The day-to-day application of corrosion preventive compounds protects metal aircraft parts and components. They prevent corrosive materials from contacting and corroding bare metal surfaces. Many of these compounds also displace water and other contaminants from the surfaces. Some also lubricate as well as protect against corrosion. Corrosion preventive compounds vary in appearance and consistency from thick, black types to light oils. Some are water displacing and others are not. Thicker compounds provide the best corrosion protection, are longer lasting, and are more difficult to remove. Thinner materials provide some lubrication and do not crack, chip, or peel, but must be removed and replaced regularly to provide continuing protection.

4.13.5 Surface Treatment. › 4.13.5.3 Chemical conversion coating is applied by brush, sponge stick…

4.13.5 Surface Treatment.

4.13.5.1 An important step in the corrosion control process is surface treatment of a metal with a prescribed chemical to form a protective film. Chemical surface treatments, properly applied, provide corrosion resistance to the metal and improve the adhesion of subsequently applied paints. These surface treatments, also known as chemical conversion coatings, chromate conversion coatings, chemical films, or pretreatments, are aqueous acid solutions of active, inorganic compounds which convert aluminum or magnesium surfaces to a corrosion-resistant film.

4.13.5.1.1 Aluminum and aluminum alloy chemical conversion materials conform to MIL-SPEC MIL-C-81706, Chemical Conversion Materials for Coating Aluminum and Aluminum Alloys.

4.13.5.1.2 Magnesium alloy chemical conversion materials conform to Aerospace Material Specification (AMS)-M-3171, Magnesium Alloy, Processes for Pretreatment and Prevention of Corrosion On.

4.13.5.1.3 Ferrous metals, stainless steel, and titanium treatment, prior to painting, are limited to corrosion removal and cleaning.

4.13.5.2 The surface should be prepared for application of the chemical conversion coatings.

4.13.5.2.1 Feather the edges of paint along the edge of areas that have been chemically stripped prior to pretreatment and repainting to ensure a smooth, overlapping transition between the old and new paint surfaces.

4.13.5.2.2 Clean the area with a fine or very fine clean abrasive mat saturated with water.

4.13.5.2.3 Rinse by flushing with fresh water. Particular attention should be given to fasteners and other areas where residues may become entrapped. At this stage in the cleaning, the surface should be without water beading or incomplete wetting, also called water breaks. A surface showing water breaks is usually contaminated with grease or oil, which will later interfere with conversion coating, sealing, and painting.

4.13.5.2.4 If the surface is not free of water breaks, re-clean the area with a solution of aircraft cleaning compound using an abrasive mat. Rinse thoroughly with water.

4.13.5.3 Chemical conversion coating is applied by brush, sponge stick moistener, or a non-atomizing sprayer to achieve a yellow-to-gold color for aluminum, usually 2 to 4 minutes, or greenish-brown, brassy, or brownish-yellow for magnesium, usually 30 seconds to 2 minutes.

4.13.5.4 Immediately rinse the part thoroughly with fresh water. Do not wipe with a rag or cloth.

4.13.6.3 There are numerous sealing compounds available with different… › 4.13.6.3.2 Silicone sealing compounds generally consist of one…

4.13.5.5 Allow the chemical conversion coated surface to dry a minimum of 30 minutes and a maximum of 4 hours before painting.

4.13.6 Sealants. Refer to MIL-SPEC MIL-PRF-81733, Sealing and Coating Compound, Corrosion Inhibitive.

4.13.6.1 Sealants are one of the most important tools for corrosion prevention and control. They prevent the intrusion of moisture, salt, dust, and aircraft fluids, which can lead to extensive corrosion. For sealants to be effective, it is critical to choose the correct sealant for a specific area or situation, and that it is applied correctly.

4.13.6.2 Sealants are useful in the following areas:

• Fuel tank;

• Pressure areas;

• Weather sealing;

• Firewalls;

• Electrical;

• Acid-resistant areas;

• Windows;

• High temperature applications; and

• Aerodynamic sealing.

4.13.6.3 There are numerous sealing compounds available with different properties and intended use. Refer to the aircraft manufacturer manual for specific information about selection of the sealing compound and proper application. Observe the warning and cautions of the manufacturer when using sealing compounds. Sealing compounds generally are divided into two major types: those requiring a curing agent and those which cure in air.

4.13.6.3.1 Polysulfide, polythioether, and polyurethane sealing compounds consist of the base, or prepolymer, and the accelerator, or curing agent. When thoroughly mixed, the catalyst cures the base to a rubbery solid. Rates of cure depend on the type of base, catalyst, temperature, and humidity. A full cure may take as long as 7 days.

4.13.6.3.2 Silicone sealing compounds generally consist of one component which cures by reaction with moisture in the air. If silicones are applied too thickly or in such a way as to prevent moisture from entering the material, they may not

4.13.6.4 Sealant application procedures: › 4.13.6.4.9 When required, prime sealant as soon as it no longer feels…

cure at all. Many silicone sealing compounds also produce acetic acid, which has a vinegar smell, while curing, and can lead to severe corrosion problems. Limit silicone sealing compounds on aircraft to those noncorrosive products conforming to MIL-SPEC MIL-A-46146, Adhesives-Sealants, Silicone, RTV, Noncorrosive (For Use with Sensitive Metals and Equipment).

4.13.6.3.3 Some sealing compounds need a special primer or adhesion promoter before applying the sealant to develop a good adhesive bond with the surface. Use only those primers or adhesion promoters recommended by the product manufacturer.

4.13.6.4 Sealant application procedures:

4.13.6.4.1 Remove corrosion, apply a chemical surface treatment, and prime all surfaces, except internal fuel tank surfaces. If the surfaces have been contaminated following surface treatment, clean the area with cleaning solvent and a clean cloth. Dry the surfaces immediately with a clean cloth. Do not allow solvents to evaporate from the surface.

4.13.6.4.2 Mask off the area being sealed to prevent sealant from contacting adjacent areas during application and post-application smooth-out. Examples of where masking may be beneficial are fillet sealing of exterior surface lap and butt seams.

4.13.6.4.3 When required by the manufacturer, apply a thin coating of an adhesion-promoting solution. Allow to dry by evaporation without touching the area for 30 minutes to 1 hour before applying sealant.

4.13.6.4.4 Spatula type sealants may be applied with a nonmetallic spatula or scraper. Avoid entrapping air. Work sealant into recesses by sliding the edge of the scraper firmly back over the recesses between taped areas next to the sealant application area. Smoothing will be easier if the nonmetallic scraper is first dipped in water.

4.13.6.4.5 If using a brush to apply a sealant, brush it on and smooth until the desired thickness is reached.

4.13.6.4.6 Applying sealant with a caulking gun will not usually require masking and is especially adaptable to filling seams or applying form-in-place gaskets.

4.13.6.4.7 Use a solid, continuous pattern to apply sealant with a spray gun.

4.13.6.4.8 Allow sealant to dry or cure per manufacturer recommendations.

4.13.6.4.9 When required, prime sealant as soon as it no longer feels tacky, then topcoat as necessary.

4.13.6.4.10 Apply faying surface sealant between the contacting surface of two or more parts. Use this sealant for all assembly and, where possible, reassembly. Where at all possible, use it in conjunction with fillet sealing. There are two types of faying surface seal installations, removable and permanent. The removable type is for access doors, removable panels, inspection plates, windows, etc. The sealant is normally applied to the substructure and a parting agent applied on the removable panel during sealant cure. The permanent type is for sealing between parts of a structure that is permanently fastened together with a high-adhesion sealant.

4.13.7 Paint Finishes and Touchup Procedures. › 4.13.7.2 Aircraft paint systems have a primer coat and topcoat.

4.13.6.5 Aircraft maintainers commonly use fillet, or seam, seals. Fillet seals cover structural joints or seams along stiffeners, skin butts, walls, spars, and longerons, and seal around fittings and fasteners. Fillet sealant should be used in conjunction with faying surface sealing and in place of it if the assembly sequence restricts the use of faying surface sealing.

4.13.6.6 Injection sealing primarily fills voids created by structural joggles, gaps, and openings. Use only sealants recommended by the aircraft or equipment manufacturer, and inject sealant into the area using a sealant gun. This method produces a continuous seal, normally impossible while fillet sealing. Clean the voids of all dirt, chips, burrs, grease, and oil before injection sealing.