Order WP 6000.6 Maintenance - Nickel Cadmium Batteries
This document is cancelled. It may have been replaced. Check the official source before relying on it.
Text read by OCR from a scanned file. Check the original, as some words may be misread.
ORDER FEDERAL AVIATION AGENCY
ORDER FEDERAL AVIATION AGENCY
Western-Pacific Region WP 6000.6
818/66 MASTER FILE
SUBJ: MAINTENANCE - NICKEL CADMIUM BATTERTES
1. PURPOSE. This Order provides information to Area Airway Facilities personnel to aid in the understanding and proper use of nickel cadmium batteries.
2. REFERENCE. Sonctonc publication, Nickel Cadmiu Batteries, by Lewis Hofstatter, Applications Engineer.
SUBJ: MAINTENANCE - NICKEL CADMIUM BATTERTES
3. BACKGROUND.
a. The present limited use of nickel cadmium batteries in the FAA can be expected to increase in the future.
b. The generally excellent performance of nickel cadmium batteries, and the proprietary pride of some manufacturers and/or assemblers of equipment using these batteries, has resulted in some misapplication and mishandling of this useful device.
c. The chief problem is proper charging procedure. The statement is frequently made that nickel cadmium batteries cannot be overcharged, but this is true only when CORRECTLY DESIGNED limited, or trickle, charge devices are used.
d. Charging methods suitable for lead-acid batteries are entirely inadequate for nickel cadmium batteries without close observation, constant attention, and knowledge of pertinent factors.
e. There is at present no practical, or readily applied, method by which the existing state of partial charge of a nickel cadmium battery can be determined. Without knowledge of this factor, high rate charging cannot be used for the sealed cells without encountering destructive gassing.
4. DISCUSSION. The subject of nickel cadmium batteries is quite comprehensively covered in the referenced Sonotone publication. Personnei concerned with nickel cadmium battery care and use can benefit from a study of this material. While this is a proprietary article, and minimizes some of the known problems, there is much basic information that can be of great value.
DistribuNon: M-1, MAF-3, RAF-2, FAF-2 (1 copy), Initiated by: WP-:444 SM-1 (2 copies), WE-430 (1 copy), 460 WE-440 (1 copy), WE-450 (1 copy)
Page 2 WP 6000.6 8/8166
Special attention should be given to the section entitled: Temperature Effects and Charge Retention. The fact of great importance developed here is that the end-of-charge voltage varies inversely with temperature change and can result in thermal runaway. This effect was strikingly demonstrated at several desert sites where vented nickel cadmium batteries were used for engine starting. The conventional lead-acid constant potential system was used for charging. The extremes of tempersture made it impossible to find any compromise rate, with the result that the batteries either discharged or boiled . violently.. It is now known that these batteries could have been used successfully if they had been charged at a constant low trickle rate. The high rate automatic charger should have been used only manually for periodic checks by a technician who could observe the end of charge indication by the start of gassing.
b. The discussions of the C/10 and C/l00 rates are particularly pertinent. ·Assemblers of instruments and equipment are not always conscious of the charging limitations and inadvertently build in rates which may prove to be excessive if used for the time intervals recommended by the instructions .for the user; for example, the Alectrs llB DBM/DBA meter.
(1) As originally furnished by the manufacturer, the meter had a charging circuit which forced 40-50 mm. into the 225 ma. battery.
(2) The instructions for charging stated, "It is strongly recommended that it be made standard operating practice to place the battery on charge every night. The battery cannot be damaged by overcharging and the inconvenience of a dead battery will thus automatically be avoided."
(3) Operation under these conditions naturally resulted in early failure of many batteries from rupture of the seals and drying out of the electrolyte. The reason is very spparent since this is & C/5 rate continued for 16 hours every night.
(4) The charging rate was subsequently corrected to a C/l0 rate by modification instructions in AF P 6500.1, CH 17, Chapter l03. However, even with this reduced rate it should be apparent that the battery cannot be charged "every night" unless it has been used all day at its normal discharge of about 20 ms. The 140% charge rule discussed in the reference should be conformed to ss nearly as is possible and practicai.
c. The cell reversal discussion will slso be enlightening to those technicians who have had batteries fail after overdischarge.
Par. 4
WP 6000.6 8/8/66 MASTER FILE Page 3
5. ACTION. Technicians responsible for maintenance of equipment which utilizes nickel cadmium batteries shall consider the referenced information and determine that the charging rates and/or charging times are appropriate for the capacity and type of battery. Where discrepancies are found, between manual operating instructions and the practical limitations of the battery, data shall be provided to support recommendations for changes to equipment or operating methods.
APPROVED WESTERN REGION AUGUST 8, 1966
APPROVED WESTERN REGION AUGUST 8, 1966
Par. 5
MASTER FILE WP 6000.6
Nickel-Cadmium Batteries
By LEWIS HCFSTATTER/ Appications Engineer, Batters D. Scnotone Corp.
This iruiy rrcaargeable and compact power sourcc has led
to the devclopment u; a wide variety of corailrss d-vices
in consumir, commercial, industrial. and mili!cr arsa:.
MASTER FILE WP 6000.6
NE of the most sigulucani do lopments in port. veloned .anv during the Second Worlc War. d uas ahit power durin th: pust pcars has heen the proruced i. ins country shortly after the war enc.d. The refinement and mass production of nickel-cad- grc.ulest cuii:nt activity and volume in nickel-caimium
mium alkaline batteries. Mary miliions of sealed and vented rechargeahle cells h:ve hecn used successfully in a tary applications. Whole fal.tlies of new cordiess products have come into being, haie. . the high perform- wide variety of consumer ommercial. indusirial, and mili- ance capabilities of the scnic nici.er-cudmium sysiem. The a brilliant future and, unt.i tic í.ei c..: becomes econom- ically practical, it seems itcis that l'.. greatest hope fer market for the truly rechurestle battery continues to bave reliabie portable rechargeat ': powc: !! e with the nicke!- cadmiúm battcry system. batte:es is uitn the sealed sintered-plate types. The bes tesumc: a the fficiency, reliahility, and coriplete lack et mantonance ir sealed nickel-cadmrum cells is ine fact that p'onatt riore than half the consumers usirg cordless appliances t. such hatteries do nor even realiz? :r at they conta:? ha:t:-:es at ali. Many manutacturers have encour- aged inis lerxlcncy by referring to the power source as ar. "energy ce!'" cr a "powerpack," because they feel tha" there may othoruise he -ome sales res:stance to a batte: :-pow- ered devi.r & psti separator or diclectric, a negu.. Th: sc sirtered-plate cell has fve main comnnents
Pocket-Plac Nickei-.admium electrolyt: :l a container. (See cnver illustra:ion.: o
Waidemar Jungner of Swen :: 1a and emplnyed an upen pocket-plate type oi c::ll. structure containing parailel rrvs of sn.:!" pockets or cham- hers to hold the acti. matcr:ais The: pockets are very ting the escape of the materia: "sicie F'olystyrene or glass plates contain nickel sal:s and the negative piates contain finely perforated to allow electrd I-ie iccess without permit- rods ure used as senarators heiwcen plates immersed in aqueous potassium hydroxide ciectrolyre. Thc positive cadmium salts. proven to be the heavy-duty work horse of the industry. hours, the cells may be encased in either plastic or sieel. Available in capacities from 10 to about 2000 ampere- They are assembied in hardwoxxi trays of convenient size 24, 32, 48, 110, and 220, but any inlermediate value can and these can then be tiered in sicel racks. Each cell deliv- ers 1.2 volts and the most common voltage units are 6, 12, also be obtained. The first rechargeatie alnu: ne hnterv was developed hy The pockei plate (Fig. 1, left) is a liat nickei-plated stce!
The vented pocket-plate nickei-cadmium battery has These batteries have an extremely low internal resistance accessrnded in a sealed cell and a lir tity ni elerrulvic is used. thus reducing mantenali. 'o. minimur: 7dt eiiminating the need tc add eithei w.'. electrnlytc. sinter.ng . tine nickci powder to a woven nickei vire screer: :S ntering involves the conversion of a soute. or earthy suhsiance into a coherent solid mass hv he.? without thoroughly melting. This not only acts as latr conductor. hut also imparts gresi strength and llexihil:!) io the plate. This results in a thin. highly porous nickel pl:que (Fig. 1. enter) which is then impregnated with n.ckei .alt solutions 'or the nositive plate and cadmium salt solut.ons ically separates the positive plate from the negative u hile for the negativc plate. holding electrotyte and permitting ions or electrical c nt to flow between the plates. The electrolyte uscd is ar: u.:- ous solution of potassium hydroxide. cover.
The cell i:. assemhled hy rolling hoth plate:. sepa. rated by the dielectric, into a tight roll or core wh'ch .: ·her Preparauc" ot positive or nepative piates reucires .he The separator. an ahsorbent dielcctric material, nicchan- The usual celi container is a nickel-piated steel cur aud
accelerated rates and. at normal temperatures. will hold and can thus deliver very high currents with little loss of voltage. Converseiy. they can also he recharged at greatly Fig. 1. Three typicel nickel-cadmium bettery plates. From left. medern pecket piate, sintered piete, snd pasted piate.
their charge for very long periods. When delivering moderate currents, they will periorm satisfactorily even at temperatures of - 40°°C. Pocket-piate vented cetls utilize an excess amount of al kaline eiectrolyte and contain vents through which evolved gases are rcicased and additional water or clectrolyte may he added, if required. for proper maintenance. They are not the lightest batteries in the world. hut they prohably are the most reliable, often providing as much as 25 years' of useful service. These hatteries are thus employed in emergency standby applications with marine. lighting. alarm, control signaling, switchgear, telephone. engine starting, as well as for auxiliary utility power systems.
Sealed Sintered-Plate Nickel-Cadmium
The sintered-plate type of nickel-cadmium cell was de-
1.4 Fig. 4 also indicates what may be expected in voltage levei 1-hour discharge rate, and 550 ma.hrs. at the 20-hour rate.
1.2 on any size cell it the discharge rate is changed from the 5-hour to the 10-minute or 1-hour rate. ·High-current capahiiily. Seuleu sintered-plate cells can 1.0 deliver high current discharges in the neighhorhoou of 10 to 15 times their S-hour rated capacity. For example, a AMP. deliver 10 amperes tor a short time. The same cell will pro- "1,2C" cell with a capacity ot 80 ma.hrs. my he used to vide a lull 16 minutes of operation at a constant discharge of 2.5 amperes (see Fig. 6A). Ordinary batteries are ruined 15 by such treatment. Fig. + shows the effect ot discharge cur- TIME IN MINUTES rent upon actual celí capacity ohtainable. Nule that the Fig. 2. Cell-discherge veltege vs time fer e type S102 ceil. This is ene-helf the sise ef e stenderd "C cell. total energy availahle (the area under the cutves) is some- what lower at high current drains. but that the voltage regulation is still excellent. Table I lists representative data on a few of the more 1.6 popular types of sealed nickel-cadmium cells. Temperature Effects & Charge Retention While their discharge performance is affected somewhat 1.2 at temperature extremes. sealed. sintered-plate nickel-cad-
VOLGE TERINAL 1.0 .6 ROOM TEMPERATURE CHARGE- 16 HR RATE 12 16 mium celts offer some advantages over other battery sys- tems in this respect. At 32*F, the cells will yield approxi- mately 90% of their roum temperature capucuty, while at 125•F they will produce T0%. The cells can uiso supply useful but reduced energy over the range cf .40to trom those encountered at room temperalures as the tem- perature is either increused or Jecreased. + 165*F. Discharge voltage levels wili decrease wnewhat
CHARGE TIME IN HOURS For best results. cells shoud he charged at ambient tem Fig. J. Termined veitege meesured during a censtent cherge. can be expected to be higher 11.55 voits) than those en- peratures berween 60* and100*F. Enu-of-charge voltages
placed into the can with the eiectrolyte and sealed. The neg- alive plate tah is welded to the bottonı ul the can: making the entire cell case the negative terminal. The entire cell assemhly is then charged, discharged. and completely in- spected hy the manufacturer of the ceil. countered at room temperatures when cells are charged at cold temperatures and can he expected to be lower (1.37 voits) at the upper extreme lemperatures. This is why sealed cells should never he charged by constant potentiai, since the cells tend to warm up juring charge and thus de-
Electricai Characteristics The ctosed-circuil volrage ot a singie nickel-cadmium ROOM
hut certain other voltage levels may also be encountered. cell. irrespective of size or shape. is nominally 1.25 volts load. At room temperature. this is i.33 volis. This repre- sents ihe normal terminal voltage oi à nickel-caumium electrode pair immersed in potassium hdruxide clectrolyte. Open-circuil velrage is thé voliage ot a celi without a End-uf-dischiarge volrage is the final voitage to which a VO S1 TENAL 1.2 1.1 1O MIN.DISCH. OSCH. SHR.0ISCH
cell is discharged. Levets helow 1.0 volt per cell should be be used because most of the cell's capucily is exhuusted at avoided where possihle. Quite often. a higher end point can 1.0 0% 25% CAPACITY IN PERCENT 50x 75% 100
voltage levels soniewhere between 1.10) voits and 1.15 volts (Fig. 2). End-of-hurge voltage is the Anal oltage across the cell Fig. 4 Discharye veitage cherocteristics of cyiindrical sesled celis fer a nummer of different rates of discherge.
at the end of charge. with charge current still towing through it. A cell piaced on constant charge soon rises to a Fig. S. The verietien ef cel capeuty with disct.erge rate. voltage of 1.40 (Fig. 3) and can climh to 1.47 volts or more. 1.43 volts is an average final voltage and a ceil is questionable if it does not retlect voltuges reasonabiy close to these. 120 Appere-holl capaciry is gencrally measured to a 1.O-volt 100 per cell end-point and is the product of discharge current and the time under load. Capacity varies with the discharge rate. Figs. 4 and 5 indicate that at a 1-hour rate the cells will yieid about 80% of their 5-hour rate. which is considered the standard carate; a somewhat higher capacity than that of the S-hour pacity of the cell. At lower rates. such as the 10- or 20-hour 20 rate is obtained. To illustrate. the "AA" size (ordinary penlight) sintered-plate cell has a nominal capacity of 510 ma.hrs. at the 5-hour rate of discharge. 430 ma.hrs. at the COMPLETE DISCHARGE- TIME IN HOURS ELECTRONICS WORLD
MASTER FILE WP 6000.6
1.4 100 2
PE 1.0 80
VOLTS .8 .6 AMP. 120 MA. CHARGE 60
VOLTS .8 .6 AMP. 120 MA. CHARGE 60
ROOM TEMP.-
150 300 450 600 750 900 20 40 60 BO 100 CAPACITY IN MILLIAMPERE-HOURS STAND TIME IN DAYS (8) Fig. 6. :A) Compariten berween capecitres of "Y, C" sizr ter twe dischorge rates. Nete 600-me. hr. cepecity et 2.5-emp. discherge. 13) Chorge-retentien
ROOM TEMP.-
crease in voltage. The charge- wiil then sunpiy increased relay across the hattery terminals which disconnects the currents, causing more ncalin. nd so or, until cel! failure load u no" ierminal voltage drops to a predetermined va:u..
results. This condition i: call "hermal runaway." ànd can be prevented only hy usir: constint-current charging. State of Charge
The sealed nickei-cadnuium cell. like ail electrochemical The state of charge is the amount of energy left in a haistorage devices, loses a percentuge oi its charge while in tery at an: given time. There is no simple, practical way of storage. At room temprrture. the cell will retain 75% nf measurink :he state of charge in a nickel-cadmium system, its capucity after a 30-day stand 1 after 60 days, and since the voltage does not refect residual capacity and the 50% of its capacitv after a 9(Luu icrind ( Fig. 6B). in any .electrolyle serves chiefly as an ion-carrier, without significase, the loss of chare is oniy ut a temporary nature and cant changes in its specific gravity. When dealing with can be regained on suhsequent charging. One of the advan- either venied or sealed nickel-cadmium batteries. if in tages of a rechargeahle sysicm is that the loss of shelf life doubt .about the state of charge, the best procedure is can be prevented hy kecping :hc cells on a trickic charge or simply to give a 14hour freshening charge at the C. (1 rate simply by recharging them he'.re heiny placed into service. or keep on trickic charge permanentiy at C:100.
Cell Reversal Charging Techniques
If a multiple-celi hattery is deeply discharged at currents Recharging sealed cells is a simple matter anu can be acmuch greater than C/10 (C = amp. hr. capacity of cell at complished in severai ways. In each case. only constant- 5-hr. rate), there is a possihiitv thar cell reversai will occur. current charging shouid he used due to the possibiity of This can happen if one cell is slightly lower in capacity than "Thermal runaway." described earlier. Because there are the others and if, during discharge, its voitage falls near some heat losses. gas evolution, and side reactions. rechirgzero while the-other cells may he at one volt or more. The ing is never 100, efficient and it is necessary to replace battery will continue to discharge through the "dead" cell, 140%x of what was removed. The standard recharge ratc is charging it in reverse. as it were. If the discharge continues at a current value of 'iu the cell capacity (C/10) íor trom long enough. the celi may reverse its polarity and he dam- 1410 16 hours. aged.
Fig. 7.A shows a typical half-wave constant-current It occasionally hecomes necessary to protect a seaied charger. Note that no filtering is required for nickcl-cadnickel-cadmium battery from the repetitive deep discharges mium chargers. since the average cell has an cnorous that might prove injurious. In some cases. the device can equivalent capacitance. The charger is actually a currentbe designed to become inoperative when the voltage drops limited device and will not really provide a truly "constant" below 1 volt per cell. At other times, the user can he in- current. since the counter-e.m.f. of the batteryrises during structed to charge whenever the power appears to weaken. charge and wili oppose the transformer e.m.i. The charge One solution is to use the appropriate zener diode across currents will be quite constant enough, however. for huteach cell to prevent it from being driven into reverse polar- tery charging and no trouhle will be encountered if the curity.
When the weakest cell reaches a reverse 0.1 voit, the rent at the end of the charge does not exceed the C/10 ratc diode will pass all the current instead of the cell, thus pre- for sintered-plate hatteries. venting damage. The correct zener diode must be able to The value of R is chosen as follows: begin conducting current at very low voltages and must 1. Multiply the number of cells by 1.45 volts to obtain possess the required current-handling capability. Such di- the counter-e.m.1. at end-of-charge. odes are often quite expensive. so simpler techniques are 2. Select transiormer with a secondary voltage that is at generally employed. These usually involve the use of a least twice this voltage.
Tobie 1. Chorocteristics of sesled colls. "AA" cells are penlight type whiie "D" ceils ere standerd flashlight type.
Size (5-hr. rate) Capacity Average (1-hr. rate) Capacity Average (constant current) Charge for 14-hours Dia. (in.) Hgt. (in.) Over-all Weight (oz.) (in milliohms) Impedance 60-cps
MA .51 amp. hr. .43 amp. hr. 50 ma. .580 1.985 0.8 22
C 1.9 1.6 150 1.022 1.925 2.6 15
D 40 3.2 400 1.333 2.385 5.5 12
F 6.5 6.0 600 1.333 3.455 8.3 7
INPUT: 117 VAG 117 VAG.
(A) (8) 47Ω C(SEE TABLE 2) wt
100,000p 117 VAC
(C) (0) Fig. 7. A greuping.of nearty censtent current de
current (or the current desired) for the value of 1, and soive (2). for R. The wattage rating of the resistor should be 2.5 to 3 times the product of E and 1. Adjustabie resistors are handy för proiotype use, because exact settings can be made. maximum anticipated current. Remember that a heavily rate the baliast resistor in the secondary winding of the age raling. It wili run cool if capable of handling twice the discharged battery will draw subetantially bigher currents transformer, others use an incandescent pilot light as a com- until its counter-e.m.f. rises. Some manufacturers incorpo- bination resistor, fuse, and charge-rate indicator.. charging can be used. If the transformer secondary is cen- ter-tapped. the double-diode circuit of Fig. 7B can be used. voltage of the transformer is just twice that required for The value for R is calculated as above, but the secondary 3. Subtract voltage from step (1) from voltage of step 4.
Use this value for E in the formula R= E/1; use C/10 The diode shouid have a conservative peak inverse voit- At higher currents and for greater efficiency, fuli-wave from a larger primary battery-he reiative voltages often work out perfectly. For example, a pair of 20 ma.hr. hear- ing-aid cells can be recharged in parallel from a singie #6 Leclanché cell. These cells may be kept on charge while another pair of celis is used in the hearing aid. At least two years of use can be obtained in this manner. event of cell abuse. A puncturabie diaphragm composes the sort of safety venting device to prevent seal failure in the top celi seal and a piercing point impinges upon the center of the diaphragm. Any gas accumulation due to excessive discharging or charging rates will cause the diaphragm to be distended upward and the point will make a small punc- ture. When the gas pressure is relieved by venting to the external atmosphere through the hole in the top cover, the diaphragm is elastically restored to.its original plane, almost closing the pierced opening.
The cell will continue to func- tion for a number of cycies but it will naturally age some- what faster than wouid an unpunctured cell. Smailer cells can sometimes be conveniently recharged Most sintered-piate seaied cells made today have some
half-wave rectification. Cycle Life & Packaging
rectifier requres four diodes and must not be operated ary and a bridge rectifier is shown in Fig. 7C. The bridge rent imbalance could damage the diodes. The same bridge can be used with a capacitor repiacing the transformer, as without the battery connected, because the resulting cur- in Fig. 7D. Due to the size of the capacitor, it is feasible oniy for smail or moderate currents. Table 2 shows some typical values for C at various charge rates. A common fuli-wave charger using an untapped:second- cycles of operation possible betore capacity drops to a pre- determined level. Cycie life is at an optimum when over- discharge is avoided, recharging is performed regulariy, and depth-of-discharge is kept as shaiiow as possibie. When are used. cycle life may be in the thousands. the charge-discharge cycles are nearly fuil, life is measur- able in hundreds of such cycles: when partial discharges Cycle life refers to the number of charge-discharge Sealed ceiis are available in capacities from 20 ma.hrs.
Table. 2. Veiues for series cepeciter C in Mig. 70. Thle to 25 ampere-hours and they can all be assembled to form
cennected directty te the pewer line, hence it shoukd be perricuier circuit hes e petestel sheck hazard es is-is. buill inte ond device with suiteble persennel presection. a variety of finished battery packs. Small disc cells are stacked to make compact cylindrical batteries. The popu- lar cylindrical celis may be packaged either in long end-
Cell Capacity Number of Cells Value of C Nominal Charging (ma.hr.) in Series (in t.) Current (ma.) to-end cylinders or side-by-side in convenient moduiar configuration; larger rectangular cells are assembled side- by-side in battery trays or enciusures.
50 1 to 5 0.12 5 Pasted or Pressed Piate 100 1 to 5 0.25 10 For many years, nickel-cadmium ceils have been made by simply pressing. under pressure, a'paste of active mate- 150 1 to 5 0.40 15 riais into a supporting matrix (Fig. 1, right) rather than by sintering. This type of cell is less expensive to produce, has 250 1 to 5 0.65 25 excellent charge retention, and gives good capacity-volume 500 1 to 5 1.40 50 efficiency. However, it has a higher internal resistance and is thus limited to low and moderate current-drain applica-
1000 1 to 5 3.25 100 tions. Pasted-plate cells are available in both cyliodrical and disc-shaped configurations; the latter can be assembled
ELECTRONICS WORLD
ELECTRONICS WORLD
:n sacks to give any desired voitage. These cells are rela. tively inexpensive compared to the sintered-plate type and MASTER FILE WP 6000.6
have a minimum average life of from one to three years.
Vented Sintered-Plate Batteries
Vented cells are produced from standard sintered plates which are made in parallel assemblies to give a rectanguiar configuration (Fig. 8). Batteries of these cells can safely deliver enormous currents with good voltage regulation. They may be fully charged in times as short as s hour over temperatures from -65° to + 165*F. The cell containers are polystyrene or nylon and are housed in stainless steel or fiberglass battery cases. No acids, noxious gases, or corrosive fumes are evoived during normai use. Because of the type of one-way vent employed, these cells can be discharged in any position, although they should be kept vertical during fast discharge to prevent loss of electrolyte. Vented sintered-piate batteries can be stored for long periods in any state of charge and will retain a charge for at least a year. The extremely long life and corrosion-resistant construçtion virtually eliminates the need for inspection or maintenance. An occasional eiectrolyte check and the addition of a little distilled water a couple of times a year is all that may he required.
If it ever becomes necessary to change a vented cell in a battery, the ceil is simply removed and replaced by a new one. This feature enables every battery celi to be used to exhaustion. Because all tbe iniernal conncctions are weided and the plates have very low resistance, puise discharges up to 40 times the cell capacity are pos- seems more suitubte. Combination circuits can be designed sibie. to charge initially at constant voltage and high current, then The vented sintered-plate nickel-cadmium batteries are taper automaticaliy to constant trickie current. extensiveiy used in military and industriai applications, in- Ar times it may be r.ecessary to charge two or more cells cluding engine starting, switchgear operation. and emer- in parallel. This can he accomplished by inserting a resistor gency standby service. Availabie in low-, medium-, and in series with each of tne cells being charged from a single high-current rate versions, they are more expensive than source.
The value of the resistor chosen must be at least 100 their sealed counterparts but have a normal life expectancy times the magnitwde of the internai resistance of each cell. of from 5 to 10 years. Vented ceils may be charged with Slight differences in ceil internal resistance thus exert a either constant voltage or constant current, whichever negligible effect.
ALKALINE-MANGANESE NICKEL-CADMIUM
ALKALINE-MANGANESE NICKEL-CADMIUM
SILVER-CADMIUM CARBON-ZINC SILVER-ZINC Battery Sources
MERCURY Acme Battery Corp., 200 Henry St., Stamford, Conn. Alkaline Batteries Co., 2278 Mora Dr., Mountain View, Cal. Bright Star Industries, 600 Getty Ave., Clifton, N. J. Burgess Battery Co., Freeport, Illinois Carbone Corp., 400 Myrtie Ave., Boonton, N. J. Catalyst Research Corp., 6101 Falls Road, Baltirxore 9. Mid. Cook Batteries Co., Denver, Colorado Delco-Remy Div., Generai Motors Corp., Anderson, Indiana Eagle-Picher Co. Chemicals Div., P.O.B.290. Jopiin, Mo. Electric Storage Battery Co., 2 Penn Center Ptaza, Philadelphia, Pa. Electrochimica Corp., 1140 O'Brien Dr., Melno Park, Cal. Generat Electric Co., Battery Prod. Sect, P.O.B. i 14, Gainesville, Florida General Eiectric Co., Ordnance Dept, 100 Plastics Ave., Pittsfield, Mass. Gould-National Batteries Inc., Alkaline Battery Div, 1st Nat. Bank Bidg., St. Paul, Minn. Gulton Industries Inc., 212 Durham Ave., Metuchen, N. J. Mallory Battery Co., Broadway & Sunnyside Lane, Tarrytown, N.Y. Marathon Battery Co., Box 298, Wausau, Wisconsin Nife Inc., Copiague, Long Island, N. Y. RCA, Electronics Components and Devices, 415 S. Fifth St., Harrison, N. J. Sonotone Corp., Battery Div., Saw Mill River Rd., Eimstord, N. Y. Telecomputing Corp., Power Sources Div., 3850 Olive St.. Denver, Colorado Union Carbide Corp., Eveready, 270 Park Ave., New York 17, N. Y." Yardney Electric Co., 40 Leonard St., New York 13, N. Y.
*Aiso makes air-depolarized types.
1