CAM 6 Rotorcraft Airworthiness; Normal Category Service Life of Main Rotors
This document is historical. It may have been replaced. Check the official source before relying on it.
Text read by OCR from a scanned file. Check the original, as some words may be misread.
UNITED STATES OF AMERICA
UNITED STATES OF AMERICA
FEDERAL AVIATION AGENCY
WASHINGTON, D.C.
For Information Only
[Reg. Docket No. 1518; Supp. No. 20] revision to Appendix A, a minimum re- PART 6—ROTORCRAFT AIRWORTHI- duction of 20 percent in the S-N test
NESS; NORMAL CATEGORY SERV- data curve has been introduced to ac- count for the scatter inherent in the
FEDERAL AVIATION AGENCY
ICE LIFE OF MAIN ROTORS results of fatigue life tests. This reduc-
Appendix A——Main Rotor Service Life Determination tion in the S-N curve makes the revised Appendix more conservative than the
present Appendix and corresponds with The policy expressed in presently ef- the procedures which are typical of fective § 6.250–1 sets forth by reference present practice by the rotorcraft to Appendix A acceptable methods of industry. compliance with the provisions of § 6.250 Since this regulatory action relates related to the establishment of service only to a statement of policy, notice and life of main rotors. public procedure hereon are unnecessary Appendix A contains those fatigue and it may be made effective on less than evaluation procedures which are accept- 30 days' notice. able methods for determining the sery- In éonsideration of the foregoing, Apice life of main rotors. However, the pendix A to Part 6 of the Civil Air Regupresent Appendix was not filed with the lations (14 CFR Part 6), is hereby r6- Office of the Federal Register and is vised to read as hereinafter set forth, therefore not presently set forth in the effective December 14, 1962: Code of Federal Regulations. The pur- (Sec. 313(a), 601, 603; 72 Stat. 752, 775, 776; posè of this regulatory action is to revise 49 U.S.C. 1854, 1421, 1423) the current Appendix by up dating the fatigue evaluation procedures in line Issued in Washington, D.C., on Decemwith current industry practice" and to ber 10, 1962. publish the revised Appendix in the Fæp- N. E. HALABY, ERAL REGIsTER. In connection with the Administrator.
(As published in the Federal Register /27 F.R. 124007 1 December 14, 1962
1168
1 APPENDIX A should define the load spectrum adequately of flight parameters that produce the most
MAIN ROTOR SERVICE LIFE DETARMINATION for each part essential to the safe operation of the rotorcraft. critical stress, loveis should be used in the fatique evaluation.
1. Introduction. The fatigue evaluation (1) The corresponding flight parameters 3. Frequency of. loading. (a) At best, procedures outlined in this appendix are (airspeed, rotor rpm, center of gravity ac- the determination of the percentage of total acceptable to the Federal Aviation Agency celerations, etc.) should also be recorded operating time associated with each flight for showing compliance with the fatigue simultaneously by approprlate methods. maneuver can only be accomplished by a evaluation requirements of CAR 6.250. How- This 1s necessary in order to correlate the statistical approach and wüll of necessity be ever, the information contained in this ap- loads and stresses with the maneuver or a function of the purpose for which the pendix is for guidance purposes only and operating condition at which they occurred. particular helicopter is intended. Obviously, is not mandatory.
(2) The instrumentation system should be a helicopter used only for crop dusting wouid (a) The rotorcraft is perhaps more di- adequately calibrated and checked periodi- have a different time distribution than one rectly affected by fatigue than any other cally throughout the flight atrain measure- used for mall or passenger "service. type of aircraft. The primary structural ment program in order to insure consistent (b) The importance of establishing repelements and systems are subject to vibratory results. Sufficient calibration data should be resentative percent of occurrences for each stresses in practically every regime of flight. submitted with the fatigue evaluation pro- flight condition cannot be overemphasized. In addition, being a highly maneuverable gram to substantiate the results obtained. Therefore, the times alloted should be based, aircraft that is capable of forward, rearward, (b) Parts to be strain-gaged.
The main on sound engineering judgment and past sideward, vertical, and rotational flight, op- rotor blades, rotor hub assembly, controls, service history if available. Table I, which erating limitations due to fatigue are pos- tall rotor, and directional control system contains suggested percent of occurrences. sible in practically all flight situations. For should be strain-gaged. For rotorcraft of along with suggested flight condition tor those reasons, it is important that special unusual or unique design, special considera- single-engine helicopters used tn normal opattention be focused on the fatigue strength tlon might be necessary to insure that all of eration, should be used as a gutde in esevaluation of the essential parts of the rotor- the essential parts are evaluated. tablishing appropriate time to be alloted for craft. (c) Flight regimes and conditions to be the varlous maneuvers. (b) Although a uniform approach to fa- investigated. The flight regimes to be in- 4. Fatigue strength.
The third phase of tigue evaluation is desirable, it is recognized veatigated in the flight strain measurement the fatigue evaluation program is the dethat in such a complex problem, new đesign program for power-on and power-off opera- termination of the fatigue strength of the features and methods of fabrication, or new tion are shown in figures I and I." For parts. Although there is information avallapproaches and confgurations may require clarity, the parameters which define these able on the fatigue strength characteristics variations and devlations from the procedures regimes are included in these figures. As of materlal specimens, the direct application described herein. Engineering judgment noted on figure I, complete coverage at 111% of such information to buft-up structures should therefore be exercised for each par- Vxm should be demonstrated for power-on is questionable. However, data from tests ticular application. operation.
However, for power-off operation, of "perfect" specimens can undoubtedly be (c) There is some question whether a com- figure I, complete coverage at 111% Vnz for an important tool in design if corrected by pletely rational method exists for the pre- mazimum and minimum design rpms need appropriate stress concentrations and safety diction of fatigue life in a built-up struc- not be obtained if points are obtained at Vxz factors. Nevertheless, there are varlous other ture subject to random loading. Neverthe- at both maximum and minimum design rpm factors which affect the fatigue strength of less, an engineering approach to the subject and at 111% Vxm at both maximum and a bullt-up structure which cannot be accan be attained through the application of minimum placarded rpms as indicated in the counted for to a reasonable degree of acthe "Cumulative Damage Hypothesis. This flgure. In addition, if the high speed points curacy.
Therefore, it is usually necessary hypothesis asserts that every cycle of stress are not obtainable at the low rpms, it is that the essential parts be subjected to reabove an "endurance limit" produces damage acceptable to vary the Vnm and 111% Vx peated load tests simulating the critical proportional to the ratio of cycles run at that speed with rotor rpm as shown in the flgures. loading conditions determined in the flight stress to the fatigue life at that stress level. (1) The determination of flight conditions strain measurement program. Special op- Laboratory tests of this hypothesis tndicate to be investigated in the flight strain meas- erational or functional characteristics which that it is reasonably valid when the stress urement program should be based on the could affect the fatigue strength should also cycles are of random magnitude.
That ls, anticipated use of the helicopter and, if be considered in the service life evaluation. stress spectra, in which all high-stress aveilable, on past service records for similar Such factors as high blade operating temmagnitudes are applied consecutively and designs. In any event, the light conditions peratures due to tip jets or turbine exhaust then all low-stress magnitudes applied, do considered appropriate for the design and impingement on the tall rotor should be not obey the hypothesis. Despite the ap- application should represent those which will considered as well as other special operating proximation invoived in the hypothesis and occur in actual operation. Suggested flight conditions. In addition, effects of special the lack of an adequate theory connecting conditions for single-engine helicopters used purpose use such as hoist and sling operathe hypothesis with more basic properties in normal operation are shown in table I, tion, spraying, surveying. etc., should be of the materials.
1t attempts to take more which should be used as a guide in making considered if appropriate to the particular factors into account than.any other method this determination. In the case of multi- type. The fatigue strength should be deterdeveloped thus far. engine helicopters, the flight conditions con- mined by either of the following methods, (d) In any rational determination of the cerning partial engine-out operation should but the testing method is recommended befatigue life of a structure, three basic fac- be considered in addition to complete power- cause of the limitations of the analytical tors must be known. These factors are: off operation. The flight conditions to be approach: (1) The stresses assoctated with the flight investigated should be submitted, in a form (a) Analytical method..
Although it has maneuvers and operating conditions ex- simllar to. table I, in connection with the been pointed out that correlating material pected; flight evaliation program. fatigue data with that of a built-up struc- (2) The frequency of oceurrence of specific (2) The severity and rapidity of control ture is difcult, it is recognized that if maxloadings expected; and movement used in control reversals, and the imum allowable stress levels are established (3) The fatigue strength characteristica of extent of blade stall investigated during the by acceptable means, and the maximum thé structure. fight strain measurement program, should stresses measured in flight are lower than 2. Flight strain measurement program. It be at least as severe as that which would these established levels, no fatigue testing is generally agreed that it is not possible at occur in service, In determining the sever- is necessary.
The following technique, based present to determine analytically the stress ity and rapidity of control movement and on the use of the Goodman diagram, is conlevels associated with normal rotorcraft oper- biade stall, consideration should be given sidered acceptable for establishing this maxiation and the correlationof occurrencē of to inadvertent overshoots during training as mum allowable stress level: critical stresses with specific maneuvers. or well as normal service. (1) Determine the endurance boundary operating conditions. Therefore, the stress (3) All flight conditions considered ap- for the perfect specimen from material data levels and occurrence of critical stresses must propriate for the particular design shouid be obtained from laboratory testa. The perfect be determined by a carefully controlled flight investigated over the complete rpm, air- laboratory specimen should be representative strain measurement program. speed, center of gravity, altitude, and weight of the material used in the actual structure (a) Instrumentation.
The instrumenta- ranges in order to determine the most criti- in regard to basic strength properties, and tlon system used in the flight strain measure- cal stress levels associated with each flight without stress concentrations. Referring to ment program should accurately measure and condition. In order to account for data fgure II, the endurance boundary for the record the critical strains and test conditiona scatter and to determine the strees levels perfect specimen may be represented by a associated with normal operation and specific present, a sufcient number of measured straight ine drawn through the yield stress maneuvers. The loçation and distribution, of strain points should be obtairied at each (point A on the, horizonal axis) and the the strain gages shouid be based on a rational flight condition. In some instances, the maximum oscillatory stress which the parevaluation of the critical stress areas.
This critical weight, center of gravity, and.alti- ticular specimen can withstand for an inmay be accomplished by a qualltative study tude ranges for the various maneuvers can be finite number of cycles (point B on the by means of brittle coatings (such as stress- based on past experience with similar de- vertical axis. The maximum oecillatory coat), by photoelastic methods, or by appro- signs. This procedure is acceptable where stress should be básed on laboratory spectpriate analytical means. In any event, the adequate flight tests are-performed to sub- mens tested without failure to at leaet 5 distribution and number of strain gages stantiate such selections. The combinations x 10 cycles for nonferrous materials or 10a
-2
cycles for ferrous materials. The line AB 5 x 10 cycles is establlshed by suitable taken to avoid the application of all high then represents the upper boundary of the means. stress levels consecutively and then all low combinations of oscillatory and steady (i1) To compensate for the scatter usually stresses. It is also désirable to keep the units stresses which the perfect specimen can associated with fatigue testing, a large num- of time at reasonably low levels. withstand without failure. ber of test specimens is desirable in estab- (3) Combination of S-N curves ánd cycli- (2) The allowable full reversal stress as lishing each S-N curve. However, most cal units. Another method of determining fadetermined in (1) should then be reduced to manufacturers cannot afford the cost and tigue strength would be by the combination account for the stress concentrations that time necessary to obtain such accuracy. of S-N curves and cyclical units. This would are present in the actual part.
The stress Therefore, a minimum of 4 test specimens involve the determination of the knee of the concentration factor chosen should be ade- which wiii establish a well deflned curve over S-N curve (endurance limit) and the fight quate to account for surface conditions, the range of oscillatory stress levels expected conditions which resulted in stresses below fabrication methods, fretting, and size and to occur in service_ is considered acceptable the endurance limit. The stresses which fáll shape efects, as well as stress concentrations in establishing each S-N curve. In order to below the endurance. limit are considered to around bolts, threads, flllets, notches, and compensate for the scatter assoclated with have no effect on the fatigue life. The rivets. The resulting line AC on the Good- fatigue testing, the mean S-N curves should method of cyclical units would then be man diagram represents the failure boundary be reduced by an appropriate factor. This applied only to those flight conditions reline for the actual part.
The selection of factor, which should be applied to the stress sulting in stresses which would cause fatigue an adequate stress concentration factor to axis, should be based·on the type of material damage. Thus, if it is established that all account for the above conditions, particularly being tested, past service experience with the level flight conditions result in stresses size and shape effects and fretting should material, and type of design. For materials which are below the endurance limit, the be based on sound engineering judgr.ent and and designs for "which service experience is actual testing would be greatly reduced. past experience. avallable, a factor of not less than 20 percent (4) Whirl stand testing., Another method (3) A factor of safety of. 3 should then be is considered acceptable. However, for new of determining the fatigue life of the essenapplied to the fatlure boundary line to estab- materials or designs this factor. should be tial parts involves the use of a whirl test lish the operating boundary line AD. The appropriately increased.
The shape of the stand on which the entire rotor assembly is
slope of line AD would be one-third of line AC. resulting reduced curve should be based on typical published S-N data and all of the tešt tested for the loads determined in the flight strain program. The fatigue life would be
(4) If the flight strain measuręments in- points should fall above the reduced curve. based on the minimum number of hours dicate that all of the operating stresses fall This curve would then represent the S-N completed without fallure for the most criti-
fatigue testing is necessary. When the below the operating boundary line (AD), no curve for use in determining the fatigue. lives. Figure IV represents this method of method is only valid when the critical loads cal stress levels determined in flight. This
measured stresses are above the operating constructing a typical S-N curve based on determined in the flight strain survey can boundary line, however, fatigue testing of the test specimens. in this example, a reduction be duplicated accurately.
actual parts is necessary. (b) Limitations of the analytical methoa. factor of 20 percent was used for explanatory purposes only. A separate S-N curve should erating conditions might involve factors (d)"Finite service ufe. Since actual op-
Caution should be exercised in. the applica- be established for each critical steady stress which cannot be ascertained by testing, it tion of the Goodman diagram method, par- level determined in the fight strain measure- becomes desirable to estabiish,an operational
numerous fllets, holes, threads, or lugs; past service experience is avallable. ticularly when the following items are involved: ratory specimens; (2) Irregularly shaped parts containing (5) Bolted or pinned connections. (1) Large parts in proportion to the labo- (3) Parts of unique design for which no (4) Parts subject to fretting; and veloped from two established S-N curves by means of Goodman or similar diagrams or ment survey. If it is desired to limit the fatigue life, a family of_ curves may be de- fatigue tests, a single S-N curve based on the in the fatigue life calculations. However, if this approach tends to unduly limit the by rational methods. Caution should be highest measured steady stress may be used exercised in extrapolating test data by means ance with the following formulas as appli- cable: fore, to compensate for these factors, the time limit, or 'service life, after which the part should be removed from service. There- service life should be established in accord- (1) Calculated sepvice llfe, L. =3,350 hours (2) Calculated service life, Lo, ≥3,360 hours Service life, L=0.75 L hours Service life, L=0.375 Le-+1,250 houra.
In view of these limitations and the dimculty of straight line Goodman diagrams, particu- (e) Infinite service Ufe. Infinite life of a in selecting an adequate overall stress con- larly from a lower alternating stress to a particular part or component may be estabcentration factor, many helicopter manufac- higher alternating stress since the results lished by demonstrating that all of the crititurers establish the operating boundary line, may be unconservative. cal operating stresses, as determinéd by the AD (fgure I) on the Goodman diagram (2) Cyclical units. The establishment of flight strain survey, are below the endurance from data based on actual tests and service fatigue iife based on cyclical unit method in- limit. This may be demonstrated by either experience.
This method is considered ac- volves the following: of the following methods: ceptable provided suicient data are used to (1) Determining by flight test the dam- (1) If all of the criticat operating stresses substantiate the allowables. aging stress levels associated with each flight fall below the operating boundary line on (c) Testing methods. The fatigue strength maneuver considered appropriate for the par- the Goodman diagram (fgure Ii) no facharacteristics of the essential parts of the ticular helicopter; tigue testing is necessary. helicopter should be determined by any of (11) Determining the number of cycles the (2) Fatigue testing at the mean stress the test methods described below or other damaging stress levels occur during each associated with the most critical meantest methods which can be shown to pro- maneuver based on the expected percentage Oscillatory stress level measured in fiight. vide similar results.
(Since lack of quality of occurrence; and No failure should ocour before 10 cýcles for control can easily result in large variations (11i) Testing of each essential part at ali of ferrous materials nor before 5 x 107 cycles in fatigue life, great care should be taken the damaging stress levels for the correspond- for nonferrous materials. The minimum to insure that production parís and assem- ing number of cycles, representing the ex- number of test specimens is dependent on blies are made with the same care as the pected maneuver history. Since the fatigue the oscillatory test. level in the following components used in any fatigue tests.) iife of the parts is unknown. beforehand, manner: (1) S-N Curves. (1) The establishment of the damaging stress levels must be covered (1) A minimum of 4 test specimens if the. a family of S-N curves is an acceptable in arbitrarlly chosen cyclical units. For ex- oscillatory level is chosen at 1.1 times the method for determining fatigue strength of ample, if cyclical units of 100 hours are critical oscillatory stress level; the essential parts.
The establishment of chosen, then reference to table I would indi- (1t) A minimum of 3 test specimens 1f the each S-N curve involves testing a sufficlent cate that the damaging stress levels and oschliatory level is chosen at 1.25 times the number of parts at the same steady stress number of cycles corresponding to 0.5 hours critical oscillatory stress level; level and varying the oscfllatory stress. at rapid increase of rpm on the ground for (1ii) A minimum of 2 test specimens 1f the Thus, in figure IV, if at a steady strees level quickly engaged clutch, 0.5 hours at jump oscillatory level is chosen at 1.5 times the
is tested until failure, fallure occurting at N. cycles, a point on the S-N curve for steady A and an oscillatory stress of level B, the part takeoff, 1.0 hours at 20% VNE for level flight, and so on throughout the maneuver history, should be included during each test- 1s chosen at 2 times the critical osciilatory critical osclllatory stress level; and (iv) One specimen if the oscillatory level
stress of level A is determined.. Additional ing unit of 100 hours. A minimum of 4 stress level. points on the S-N curve representing a steady specimens should be used and the fatigue (f) Extension of service life. The followstress of level A may be determined by choos- life of the part or component should be based ing conditions should be met to extend serving a different osclllatory stress level and on the smallest number of completed units. ice life beyond the initial retirement life testing the part to fallure. If no fallure oc- Thus, if the. smallest number of completed established in accordance with equation (2) curs for a specific loading condition, after 10a units for the 4 test specimens 1s 14, then the of paragraph (d) of this section.
stress level. However, in the case of nonfer- rous materials, it is acceptable to test to 10 cycles for nonferrous materials, the part can be considered to have infinite life at that cycles for ferrous materlals or after 5 x 10 Cumulative Damage Hypothesis on which dom magnttude. Therefore, if the cyclical fatigue life for this part would be based on 1400 hours. It should be noted that the this method is based has been found to be valid only when the stress cycles are of ran- spected for wear, fretting, cracking. etc., by which represent an adequate sampling of tial rettrement lfe. operation should successfully reach the ini- (1) A sufcient number of identical parts (2) The parts should be thoroughly in-
cycles provided the extension of the curve to unit procedure is adopted, care should be appropriate methods.
3
If these conditions have been satisfled and The summation of the individual percent- TABLE I—Continued the-parts found to be free from defects, an increase in service life might be granted. stress level is shown in column 7. There- ages of life used per hour for each dāmaging PERCENT OCCURRENCE—COntinUed The upper limit of service life which might fore, by equation (2), the calculated service (h) Right turns—30, 60, 90%
life. It is advisable to approach the 75 per- cent figure in several increments of life is 75 percent of the demonstrated fatigue be granted under these extension provisions life of thls part would be Lc= 100 0.15289 100 =654 hours (1) Left turns—30, 60, 90% (D) Climb (takeoff/power)- VNE-- VNE- 3.0 2.0 3.0
extension. 5. Sample calculation based on S-N.data. The service life of this part would be, as explained in paragraph (d) of section 4. (k) Clmb (max. continuous power) -_- 4.0 The Cumulative Damage Hypothesis states that every cycle of stress above an endurance L=0.75×654 (1) Change to autorotation from power-on flight limit produces damage proportional to the L=490 hours 30, 60, 90 % VNE-- 1.5 ratio of cycles run at that stress to the fa- A summary of the measured stress and per- (m) Partial power descent tigue life at that stress level. Thus, if a cent life used at the various flight conditions (including condition of part is subjected to random loading for n1 should be submitted with the fatigue evalu- zero flow through rotor) – 2.0 cycles at a stress level of S, n2 cycles at S2. ation program in a form similar to table . (n) Cyclic and collective puiln3 cycles at S, and so on, and if N1, N2. ups from Ievel flight__-- 1.0 N3 are the corresponding number of cycles TABLE I (o) Lateral reversals at VH--- .6 to failure for each stress level, then failure PERCENT OCCURRENCE (P) Longitudinal reversals at will'occur with the summation: .5 I. Ground conditions___. 1.5 (q) Rudder reversals at VH--- .5 N+N+N+N ni =1, or Ni =1 (a) Rapid increase of rpm on ground to quickiy en- (r) (s) Landing approach-. Sideward fight_. 3.0 .5
pressed by life of a part subjected to random loading can be determined if the percent of life used per hour at each damaging stress level is at each damaging stress level, can be ex- Using this expression, the calculated 'service known. The percent of life used per hour II. Hovering. (c) Jump takeoff_ (b) Taxiing with full cyclic (a) Steadyhovering-- (b) Lateral reversai. (c) Longitudinal reversal control_. gageclutch_. 0.5 .5 .5 .5 .5 5 2.0 iv. Autorotation-power off. (b) Rapid power recovery from (d) Left turns—30, 60, 90% (a) Steady forward fight_ (t) (c) Rearward flight Right turns—30. 60, 90% VNE- autorotational flight_ 2.0 1.0 .5 .5 9.0
where: 1= an N .-(1) II. Forward flight power on- (a) (d) Level flight—20% VNE-- Rudder reversal... 1.0 .5 87.5 (e) (t) Longitudinal reversale__- Lateral reversals_ VNE-- 1.0 .5 .5
1=percent of life used per hour at the damaging stress level; (b) (c) Level flight-60% VNE---- Level fllght40% VNE-- 18.0 3.0 (h) Cyclic and collective pul- (g) Rudder reversals. .5 a=percent of total operating time al- (d) Level fight 80% VNE---- 25.0 ups__ 1.0
which the damaging stress level was Iotted to the flight condition during recorded; (f) (e) Maximum level flight (but VNE not greater than VNE) -- 15.0 3.0 (1) Landings flares) (ipcluding 2.0
N= total number of cycles of the damag- (g) 111% VNE- .5 100.0 100.0 n=number of cycles the damaging stress ing stress level at fatlure; and TABLE II-DETEDMINATON OF SERVIE LuF level occurs per hour. (Sample Caleulation)
Thus, the calculated service lfe, Le. of a particular part or component subjected to a .1 2 3 4 5 6 7
randum number of damaging stress leyels, would be Flight condition occurrence Percent Critical Oscillatory Cycles to fallure Cyclea Percent of
1+12+13+..1= 100 21 100 -(2) Table I Table I Critical steady stress oscillatory stress Cycles/Er stress Figure V per hour life used
A sample calculation illustrating this method for determining the calculated service life I.(8) 0.5 Level A. 1900 23,200 1s shown in table II. In this example, the do 2100 23,200 peak steady and vibratory stress levels asso- ciated with each maneuver have been as- do. do do. 2600 2300 9600 23, 200 28,200 23,200 ,000,000 sumed to occur for the duration of the 5 do. 10500 23,200 8,200, 000 .00362
maneuver (columns 3 and 4). In addition, the cycles of oscillatory streas per hour also has been conservatively assumed at the max- III 18.0 3.0 1.0 5 do. do. 6500 5100 3400 7700 23,200 23,200 23,200 23,200 imum level throughout the flight spectrum 25.0 do. 8100 23,200
the service iife unduly, it is acceptable to use the actual measured stress level distributions (column 5). If this procedure tends to limit 15.0 3.0 8.0 do. 11200 8900 9100 8380 23,200 23,200 23,200 23,200 16,000,000 8400, 000 7,400,000 .00829 .00157 .02900 .02175
if proper account of possible varlations is 3.0 do. 11400 23,200 .03093 provided by repeated maneuvers. The num- ber of cycies to faflure for each damaging 40 2.0 15 do. do. do. 10900 9900 7808 23,200 23,200 23,200 4,100,000 .02263 .01719 stress level (column 6) was determined from 20 do... 6700 23,200 flgure V. As an example, consider flight 10 do.. 9700 7800 23,200 23,200 4,800,000 00483 condition II(c) of. table II. The percent of do.-- 7900 23,20 total operating time (a) considered at this maneuver is 0.5%, the damaging oscillatory a0 6700 7300 6700 23,200 23,200 23,200
stress level is 10,500 psi, the number cycles of damaging stress per hour (n) is 23,200 IV (b) 2.0 5 do. 7100 7900 9700 23,200 23,200 23,200 4,800,000 .00242 and the number of cycles to fallure (N) from (c) 10 do. 9308 23,200 6,300,000 00368 Then by equation (1) the percent of life the S-N curve (fgure V) is 3,200,000 cycles. (d) (e) 1.0 do. do. do. 9900 6800 6100 23,200 23,200 23,200 4,100,000 .00568
used per hour at this damaging stress level would be (b) (1) 20 1.0 5 do.. do. do. 5900 7600 7900 23, 200 23,200 23,200
1= an0.5×23,000 N= 3,200,000 =0.00362 Total. 100.0 .15289
FIGURE I POWER ON Rotor R.P.M. Airspeed Envelope Note: Dashed lines indicate test boundaries. Cross-hatched areas indicate operating regimes.
VNE (6.711)-
Max. design or demonstrated rpm 6.103 6.204
ROR RPH Normal operating rpm
Min, design or demonatrated rpm 6.103, 6.204 2111% VNE (6.110, 6.204)
AIRSPEED
5 POWER OFT Rotor R.P.M. Airspeed Envelope
Max.design_or demonstrated rpm TE (6.711) S 6.103, 6.204 Max. placard rpm 6.103, 6.713 (95% max, design)
H H
Min. placard rpm
Min, design or demonstrated rpm 6,103, 6.204 6.103, 6.713 (105% min, design) S11I% VNE (6.10,6.204)
AIRSPEED
FIGURE III
FIGURE III
OSOCSS SCTTESS Failure Boundary
D Operating Boundary (D=1/3C)
Steady Stress
FIGURE IV
Steady Stress Level - A
B
.Test Data Curve
No failure at required number of cycles (5 x 107) 20% Reduction
N
20000
18000
16000
14000
12000
10000
8000
6000
4000.
2000
FIGURE V
Steady Stress - Lerel
FIGURE V
Patigoe Test Data
20% redaction
206 108 CYCLES [F.R. Doc. 62–12328; Filed, Dec. 13, 1962; 8:45 a.m.}