AC 150/5320-17 Airfield Pavement Surface Evaluation and Rating Manuals
Provides guidance on understanding and rating the surface condition of flexible and rigid airfield pavements and provides a simple system to visually rate pavement condition. Because of the size of this document, it is available as one complete file (see Complete) or as three smaller files (see Parts 1-3).
This document is cancelled. It may have been replaced. Check the official source before relying on it.
U.S. Department of Transportation Federal Aviation Administration
Advisory Circular
Subject: AIRFIELD PAVEMENT SURFACE EVALUATION AND RATING MANUALS
Date: 7/12/04 Initiated by: AAS-100
AC No: 150/5320-17 Change:
1. PURPOSE. This Advisory Circular (AC) provides guidance on understanding and rating the surface condition of flexible and rigid airfield pavements. It describes types and causes of distress and provides a simple system to visually rate pavement condition on a scale ranging from excellent to failed. 2. BACKGROUND. The Federal Aviation Administration (FAA) evaluated options for improving the quality of information available to the Agency on airfield pavement conditions in response to Section 160 of the Wendall H. Ford Aviation Investment and Reform Act for the 21st Century (P.L. 106–181). The evaluation resulted in selecting an existing inexpensive pavement condition rating system to adapt for use on airfield pavements. The rating system is modeled after the University of Wisconsin's Pavement Surface Evaluation and Rating System (PASER). The rating system is meant as a source of information for rating pavements under the airport safety data program. The manuals will also assist airport managers in understanding the surface condition of airfield pavements. These manuals were produced for the FAA by Engineering Professional Development, College of Engineering, University of Wisconsin–Madison. 3. APPLICATION. The FAA recommends the information and procedures contained in the manuals for use by airport staff and consultants directly or in combination with additional testing and data collection in a more comprehensive pavement maintenance management system. DAVID L. BENNETT Director, Office of Airport Safety and Standards
The information in this AC is not intended to decide the need or timeliness for pavement rehabilitation projects. These decisions should be determined as a result of more technical investigations that may include a detailed pavement condition index (PCI) study. The manuals will help provide a degree of uniformity to field observations made by individuals collecting data for the Airport Master Record (FAA Form 5010). The data element description for Surface Type/Condition (Data Element 33 of the National Airspace System Resources database) has been revised to incorporate information from this AC. The manual for asphalt airfield pavements is included in this AC as Appendix 1. The manual for concrete airfield pavements is included as Appendix 2. 4. RELATED READING MATERIAL. AC 150/5380-6, Guidelines and Procedures for Maintenance of Airport Pavements, and AC 150/5380-8, Handbook for Identification of Alkali- Silica Reactivity in Airfield Pavements provide additional guidance and technical information for identifying distresses in airfield pavements. 5. ONLINE AVAILABILITY. To view and download this AC, visit the FAA Web site at http://www.faa.gov/arp/150acs.cfm.
APPENDIX 1--ASPHALT AIRFIELD PAVEMENT SURFACE EVALUATION AND RATING MANUAL
APPENDIX 1--ASPHALT AIRFIELD PAVEMENT SURFACE EVALUATION AND RATING MANUAL
Pavement Surface Evaluation and Rating PASER Manual
Asphalt Airfield Pavements
RATING
5
RATING
3
RATING
1
This manual is intended to assist airfield managers in understanding and rating the surface condition of asphalt pavement. It describes types and causes of defects and provides a simple system to visually rate pavement condition.
Produced for the Federal Aviation Administration by Engineering Professional Development, College of Engineering, University of Wisconsin-Madison.
Contents
Introduction 2
Evaluating pavement condition 3
Surface defects 4
Surface deformation 5
Cracks 7
Patches and potholes 12
Rating pavement surface condition 14
Rating system 14
Rating 5 — Excellent 15
Rating 4 — Good 16
Rating 3 — Fair 18
Rating 2 — Poor 20
Rating 1 — Failed 22
Practical advice on rating airfield pavements 23
Airfield Pavement Inventory inside back cover
Donald Walker, P.E., University of Wisconsin–Madison, author Lynn Entine, Entine & Associates, editor Susan Kummer, Artifax, designer
PASER Manual
Pavement Surface Evaluation and Rating
Asphalt Airfield Pavements
An airport manager’s goal is to use available funds to provide a safe and economical pavement surface—no simple task. It requires balancing priorities and making difficult decisions in order to manage pavements. General aviation airfield pavements are often managed informally, based on the staff’s judgment and experience. While this process is both important and functional, using a slightly more formalized technique can make it easier to manage pavements effectively.
Experience has shown that there are three especially useful steps in managing pavements:
1) Inventory all pavements.
2) Periodically evaluate the condition of all pavements.
3) Use the condition evaluations to set priorities for projects and evaluate alternative treatments.
A comprehensive pavement management system involves collecting data and assessing several pavement characteristics: roughness, surface distress (condition), surface skid characteristics, drainage, and structure (pavement strength and deflection). Planners can combine this condition data with economic analysis, to develop short-range and long-range plans for a variety of budget levels. However, general aviation agencies may lack the resources for such a full-scale system.
Since surface condition is the most vital element in any pavement management system, managers may use the simplified rating system presented in this manual on asphalt airfield pavements to evaluate their asphalt pavements. A PASER manual for concrete airfield pavements is also available (see references, page 24).
PASER — Pavement Surface Evaluation and Rating Asphalt Airfield Pavements
PASER uses visual inspection to evaluate pavement surface conditions. The key to a useful evaluation is identifying different types of pavement distress and linking them to a cause. Understanding the cause for current conditions is important in selecting an appropriate maintenance or rehabilitation technique.
There are four major categories of common asphalt pavement surface distress:
Surface defects Raveling, flushing, polishing.
Surface deformation Rutting, distortion — rippling and shoving, settling, frost heave.
Cracks Thermal, reflection, slippage, joint/ edge, block, and alligator cracks.
Patches and potholes
Deterioration has two general causes: environmental due to weathering and aging, and structural caused by repeated traffic loadings.
Obviously, most pavement deterioration results from both environmental and structural causes. However, it is important to try to distinguish between the two in order to select the most effective rehabilitation techniques.
Evaluating pavement condition
The rate at which pavement deteriorates depends on its environment, traffic loading conditions, original construction quality, and interim maintenance procedures. Poor quality materials or poor construction procedures can significantly reduce the life of a pavement. As a result, two pavements constructed at the same time may have significantly different lives, or certain portions of a pavement may deteriorate more rapidly than others. On the other hand, timely and effective maintenance can extend a pavement’s life. Crack sealing and surface treatments (such as slurry seal) can reduce the effect of moisture in aging of asphalt pavement.
With all of these variables, it is easy to see why pavements deteriorate at various rates and why we find them in various stages of disrepair. Recognizing defects and understanding their causes helps us rate pavement condition and select costeffective repairs. The pavement defects shown on the following pages provide a background for this process.
Periodic inspection is necessary to provide current and useful evaluation data. It is recommended that PASER ratings be updated every year.
EVALUATION — Surface Defects 4
SURFACE DEFECTS
Raveling
Raveling is progressive loss of pavement material from the surface downward, caused by: stripping of the bituminous film from the aggregate, asphalt hardening due to aging, poor compaction especially in cold weather construction, or insufficient asphalt content. Slight to moderate raveling has loss of fines. Severe raveling has loss of coarse aggregate. Debris from raveling may damage aircraft. Protect pavement surfaces from the environment with a surface treatment or an overlay if additional strength is required.
SURFACE DEFECTS
Polishing
Polishing is a smooth slippery surface caused by traffic wearing off sharp edges of aggregates. Pavement grooves may also be worn away. Repair with surface treatment or thin bituminous overlay using skid-resistant aggregate.
Flushing
Flushing is excess asphalt on the surface caused by a poor initial asphalt mix design or by paving or sealcoating over a flushed surface. Repair by overlaying with properly designed asphalt mix or sealcoat.
Slight raveling. Small aggregate particles have worn away exposing tops of large aggregate.
Moderate to severe raveling. Erosion further exposes large aggregate.
Severe raveling and loss of surface material.
Polished, worn aggregate needs repair.
Flushing. Dark patches show where asphalt has worked to surface.
▼
▼
▼
▼
▼
EVALUATION — Surface Deformation 5
SURFACE DEFORMATION
SURFACE DEFORMATION
Rutting
Rutting is displacement of material, creating channels in wheelpaths. It is caused by traffic compaction or displacement of unstable material. Severe rutting (over 2”) may be caused by base or subgrade consolidation. Repair minor rutting with microsurfacing or overlays. Severe rutting requires milling the old surface or reconstructing the pavement before resurfacing. Base or subgrade improvement may be necessary if rutting is related to poor base or subgrade conditions.
Even slight rutting is evident after a rain.
Severe rutting over 2” caused by poor mix design.
Severe rutting caused by poor base or subgrade.
▼
▼
▼
EVALUATION — Surface Deformation 6
Distortion
Shoving or rippling is the displacement of surfacing material. It can develop when the asphalt mixture is unstable because of poor quality aggregate or improper mix design. Repair by milling smooth and overlaying with stable asphalt mix.
Other pavement distortions may be caused by settling, frost heave, etc. Patching may provide temporary repair. Permanent correction involves removal of unsuitable subgrade material and reconstruction.
Minor settlement over sealed crack.
▼
Heavy traffic has shoved pavement into washboard ripples and bumps.
▼
Frost heave damage from spring break-up.
▼
Severe settlement of patch.
▼
Significant settlement (over 2”) and cracking adjacent to sealed crack.
▼
Severe settling from utility trench.
▼
EVALUATION — Cracks 7
CRACKS
Thermal cracks
Thermal cracks are often regularly spaced. The cause is movement due to temperature changes and hardening of the asphalt with aging.
Thermal cracks will initially be widely spaced (several hundred feet apart). Additional cracking will occur with aging until they are closely spaced (within several feet). These usually begin as hairline or very narrow cracks; with aging they widen. If not properly sealed and maintained, secondary or multiple cracks develop parallel to the initial crack. The crack edges can further deteriorate by raveling and eroding the adjacent pavement.
Help prevent water intrusion and damage by sealing cracks as soon as they appear. Routing and cleaning the crack will improve the performance of crack sealant.
Differential thermal stress can also cause cracking. Pavement marking paint and sealcoats using materials with significantly different thermal
Water enters unsealed cracks softening pavement and causing secondary cracks.
Open crack – 1⁄2” or more in width.
Pavement ravels and erodes along open cracks causing deterioration.
Tight cracks less than 1/4” in width.
▼ ▼ ▼ ▼
Widely spaced, well-sealed cracks.
▼
Failed sealant.
▼
Pavement marking may cause thermal stress and lead to surface cracking.
▼
Sealed cracks, some closely spaced.
▼
Severe thermal cracking in coal tar sealant.
▼
EVALUATION — Cracks 8
properties can create surface cracking.
Reflection cracks
Cracks in overlays reflect the crack pattern in the pavement underneath. They are caused by movement in the underlying pavement due to temperature change. This movement creates very large stress in the overlay. Therefore, they are difficult to prevent and correct.
Slippage cracks
Crescent or rounded cracks caused by slippage between an overlay and an underlying pavement. Slippage is most likely to occur at locations where traffic is stopping and starting. Repair by removing the top surface and resurfacing using a tack coat.
Cracks reflected
through bituminous
overlay.
Hairline cracks reflected through
sealcoat.
Loss of bond between pavement layers allows traffic to break loose pieces of surface.
▼
▼
▼
EVALUATION — Cracks 9
Paving joint and edge cracks
Paving joint cracks are caused by inadequate bonding and poor compaction of the joint during construction. They may also be caused by reflection of poor joints in the underlying pavement. Cracks within one foot of the edge are caused by insufficient shoulder support, poor drainage, or frost action. Cracks usually start as hairline or very narrow, widening and eroding with age. Without crack filling, they can ravel, develop multiple cracks, and become wide enough to require patching.
Sealing cracks will help reduce moisture penetration and prevent further subgrade weakening. Paving joints. Slight crack on joint near center. Open joint on right side.
Severe cracking and edge
distress.
First stage of wheelpath cracking caused by heavy traffic loads.
▼
▼
Edge cracking in asphalt along concrete slab.
▼
▼
Partially open 1⁄4” paving joint.
▼
EVALUATION — Cracks 10
Block cracks
Block cracking is interconnected cracks forming large blocks. Cracks usually intersect at nearly right angles. Blocks may range from one foot to approximately 10’ or more across. The closer spacing indicates more advanced aging caused by shrinking and hardening of the asphalt over time. Apply surface treatments during early stages to reduce weathering of the asphalt caused by exposure to the sun, moisture and freezing. Overlay or reconstruction is required in the advanced stages.
Right angle cracking
forms blocks.
Large blocks with open cracks
filled with grass.
▼
▼
Small blocks
with open
cracks.
▼
EVALUATION — Cracks 11
Alligator cracks
Interconnected cracks forming small pieces ranging in size from about 1” to 6”. This is caused by failure of the entire pavement due to traffic loading (fatigue) and usually due to inadequate base or subgrade support. Repair by excavating and replacing failed subgrade base and surface. Large areas require reconstruction. Improvements in drainage may often be required.
Alligator crack pattern. Tight cracks and one patch.
Alligator cracking near pavement edge.
Alligator cracking and pothole.
▼ ▼ ▼
EVALUATION — Patches and Potholes 12
PATCHES AND POTHOLES
Patches
Original surface repaired with new asphalt patch material. Indicates a pavement defect or utility excavation which has been repaired. Patches with cracking, settlement or distortions indicate underlying causes remain. Repair or reconstruction are required when extensive patching shows distress.
PATCHES AND POTHOLES
Typical repair of utility excavation.
Patch in good
condition.
Patched
area in
poor condition.
Overlay repair with edge raveling
and cracks.
▼
▼
▼
EVALUATION — Patches and Potholes 13
Potholes
Holes and loss of pavement material are caused by traffic loading, fatigue and inadequate strength. Often combined with poor drainage, this can create dangerous pavement debris. Repair by excavating or rebuilding localized potholes. Reconstruction required for extensive defects.
Complete pavement failure.
Large pothole and dangerous loose debris.
Shallow pothole.
▼
▼
▼
With an understanding of surface distress, you can evaluate and rate asphalt pavement surfaces. The rating scale ranges from 5–excellent condition to 1–failed. Most pavements will deteriorate through the phases listed in the rating scale. The time it takes to go from excellent condition (5) to complete failure (1) depends largely on the quality of original construction, age, and the amount of heavy traffic loading.
Once significant deterioration begins, it is common to see pavement decline rapidly. This is usually due to a combination of loading and the effects of additional moisture. As a pavement ages and additional cracking develops, more moisture can enter the pavement and accelerate the rate of deterioration.
Rating pavement surface condition
Rating 5 – Excellent No maintenance required
Rating 4 – Good Minor routine maintenance, crack sealing
Rating 3 – Fair Preservative treatments, crack sealing and surface treatment
Rating 2 – Poor Structural improvement and leveling (patching then overlay)
Rating 1 – Failed Reconstruction
Rating system
Surface rating
Visible distress* General condition/ treatment measures
None, or initial thermal cracks, all narrow (less than 1⁄8”) 5 Excellent
Additional thermal cracking. Cracks generally spaced more than 50’ apart. Less than 10% of cracks and joints need sealing. Minimal or slight raveling. No distortion. Patches in good condition. 4 Good
Moderate raveling. Thermal cracks and joints generally spaced less than 50’ apart. Crack sealing or repair of sealant needed on 10%-25% of cracks or joints. Edge cracks along 10% or less of pavement edges. Block crack pattern with cracks 6’-10’ apart. Isolated alligator cracking and poor patches. Minor distortion or crack settlement less than 1”.
3 Fair
3 Fair
Frequent thermal cracks. Wide cracks and joints with raveling in cracks. Deterioration along more than 25% of cracks. Edge cracks on up to 25% of pavement edges. Block cracks spaced 5’ apart or less. Alligator cracking or poor patches cover up to 20% of surface area. Distortion or settlement 1“-2”.
2 Poor
2 Poor
Widespread, severe cracking with raveling and deterioration. Alligator cracking and potholes over 20% of the area. Distortion over 2”.
New pavement less than 5 years old. No maintenance or isolated crack sealing required.
Recent sealcoat or pavement over 5 years old. Seal open cracks or joints and replace sealant where needed.
Seal open cracks and joints. Replace failed sealant. Apply new surface treatment or thin overlay. Minor patching and joint repair.
Needs significant crack sealing plus patching and repair on up to 25% of pavement surface. Overlay entire area with structural overlay.
Condition may be limiting service. Needs reconstruction. 1 Failed
* A given pavement segment may only have one or two types of distess rather than all of the types listed for a particular rating.
Look at the photographs which follow and become familiar with the descriptions of the individual rating categories. To evaluate an individual pavement segment, first determine its general condition. Is it relatively new, toward the top end of the scale? In very poor condition and at the bottom of the scale? Or somewhere in between? Next, think generally about the appropriate maintenance method. Use the outlined rating categories.
Finally, review the individual pavement distress and select the appropriate surface rating. A given pavement will likely not have all of the types of distress listed for any particular rating. It may have only one or two types.
In addition to indicating the surface condition of a pavement, a given rating also includes a recommendation for needed maintenance or repair. This feature of the rating system facilitates its use and enhances its value as a tool in ongoing airfield pavement maintenance.
Rating pavement surface condition 15
RATING 5
RATING 5
EXCELLENT — No maintenance required or isolated crack sealing.
New pavement less than 5 years old. No visible distress or initial thermal cracks, all less than 1⁄8”.
New pavement.
▼
Recent overlay. Sealed joint.
▼
Rating pavement surface condition 16
RATING 4
GOOD — Seal open cracks or joints.
RATING 4
Recent sealcoat or pavement over 5 years old. Additional thermal cracking. Cracks spaced 10’-20’ apart. Open cracks and joints need sealing on less than 10% of cracks. No distortion and patches in good condition.
Recent sealcoat.
▼
▼
Cracks sealed.
No distortion. Slight raveling.
▼
Pavement more than 5 years old. No patches or distortion. Schedule routing
and sealing for isolated open joints.
Rating pavement surface condition 17
Cracks widely spaced and sealed.
▼
Joints would benefit from sealing.
▼
▼
Old sealant is leaking. Needs replacement at isolated locations.
Rating pavement surface condition 18
RATING 3
RATING 3
FAIR — Seal open cracks and joints. Apply new surface treatment or thin overlay. Minor patching and joint repair.
Moderate raveling. Thermal cracks and joints, generally spaced less than 50’ apart. Crack sealing or repair of sealant needed on 10%-25% of cracks or joints. Edge cracks along 10% or less of pavement edges. Block crack pattern with block cracks 6’-10’ apart. Isolated alligator cracking and poor patches. Minor distortion or crack settlement less than 1”.
Thermal cracks
less than 10’
apart. Slight
raveling.
Open cracks need sealing.
▼
▼
Several patches in
good condition.
▼
Worn sealcoat
needs new
surface treatment.
▼
Rating pavement surface condition 19
Moderate raveling. Joint needs sealing.
▼
Pavement settlement at crack less than 1” deep.
▼
Moderate raveling. Needs surface treatment soon.
▼
Edge cracking at several locations.
▼
Joint sealant needs replacement at several locations. Follow with new surface treatment on apron.
▼
Rating pavement surface condition 20
RATING 2
RATING 2
POOR — Needs significant crack sealing plus patching and repair on up to 25% of pavement surface. Use structural overlay over entire area.
Frequent thermal cracks. Wide cracks and joints with raveling in cracks. Deterioration along more than 25% of cracks. Edge cracks on up to 25% of pavement edges. Block cracks spaced 5’ apart or less. Alligator cracking or poor patches cover up to 20% of surface area. Distortion or settlement 1”-2”.
▼
▼
▼ ▼ ▼
Severe raveling. Wide cracks with no sealant.
Multiple cracks open
and deteriorated
Numerous cracks with
settlement over 1”.
▼
Block cracking with cracks less than 5’ apart.
▼
Patch in poor condition.
Rating pavement surface condition 21
Needs overlay.
▼
More than 25% of crack sealant needs replacement. Minor settlement over cracking.
▼
Sealant repair needed on more than 25% of cracks. ▼
Edge cracking on up to 25% of the pavement.
▼
Repair broken pavement and apply overlay. ▼
Rating pavement surface condition 22
RATING 1
RATING 1
FAILED — Condition may be limiting service. Needs reconstruction.
Widespread, severe cracking with raveling and deterioration. Alligator cracking and potholes over 20% of the area. Distortion over 2”
▼
▼
▼
Over 25% alligator cracking.
Severe cracking and deterioration.
Extensive alligator cracking. Poor patches.
▼
Failed patch. Settlement over 2”.
▼
Extensive failed
pavement and debris.
Inventory and field inspection
Most airport owners routinely observe pavement conditions as a part of their normal work. However, an actual inspection means looking at the entire system as a whole and preparing a written summary of conditions. This inspection has many benefits over casual observations. It can be helpful to compare pavement features as a whole system so ratings and maintenance decisions can be more consistent.
An inspection also encourages a review of specific conditions important in pavement maintenance, such as drainage, adequate strength, and safety.
A simple written inventory is useful in making decisions where other people are involved. You do not have to trust your memory, and you can usually answer questions in more detail. Having a written record and objective information also improves your credibility with the funding agencies.
Finally, a written inventory is very useful in documenting changing pavement conditions. Without records over several years, it is difficult to know if conditions are improving, holding their own, or declining.
A sample inventory form is shown on the inside back cover. It is very helpful to collect background information on each feature. Pavement thickness, age, and major maintenance are examples of helpful information.
Annual budgets and long range planning are best done when based on actual needs as documented with a written inventory.
Pavement features
Inventory and pavement condition data are normally organized by dividing the pavements into segments or features.
A plan or aerial photo of the entire airfield is most helpful in identifying these individual features. Runways, taxiways and aprons should be considered as separate categories. Within each category, the pavement should be separated into features with similar construction. For example, pavements with different thickness, age, or type of construction should be rated separately.
A runway may be all one feature if conditions are similar. However, if parts of the runway have significantly different construction details or condition, then separate features will make the rating more logical and useful.
Each taxiway, can be considered a separate feature. You may combine several sections of taxiway if conditions are similar.
Apron areas can be separated into features according to the areas they serve. For example, aprons serving a terminal, hangers, tie-down area, or fueling area would be separate features. Areas in different conditions may also be separated into features.
Averaging and comparing sections
No pavement feature is entirely consistent. Also surfaces in one section may not have all of the types of distress listed for any particular rating. They may have only one or two types.
The objective is to rate the condition that represents the majority of the pavement feature. Small or isolated conditions should not influence the rating. It is useful to note these special conditions on the inventory form so this information can be used in planning specific improvement projects. For example, some spot repairs may be required.
Occasionally surface conditions vary
significantly within a feature. For example, short sections of good condition may be followed by sections of poor surface conditions. In these cases, it is best to rate the feature according to the worst conditions and note the variation on the form.
The overall purpose of condition rating is to be able to compare each feature relative to all the other features in your airport pavement system. On completion you should be able to look at any two pavement features and find that the better surface has a higher rating.
Assessing drainage conditions
Moisture and poor pavement drainage are significant factors in pavement deterioration. Some assessment of drainage conditions during pavement rating is highly recommended. While you should review drainage in detail at the project level, at this stage simply include an overview drainage evaluation at the same time as you evaluate surface condition.
Consider both pavement surface drainage and lateral drainage (ditches or storm sewers). Pavement should be able to quickly shed water off the surface. Ditches should be large and deep enough to drain the pavement and remove the surface water efficiently into adjacent waterways.
Look at the crown and check for low surface areas that permit ponding. Runways and taxiways should have approximately a 1.5% cross slope or crown across the pavement. Apron areas require positive drainage and often include storm drainage systems. Maintenance of the entire drainage system is critical. Ditches, subsurface drains and outlets should be inspected and cleaned regularly.
Practical advice on rating airfield pavements
technique.
Consider future traffic projections, original construction, and pavement strength since these may dictate a more comprehensive rehabilitation than the rating suggests.
Summary
Using funds most efficiently requires good planning and accurate identification of appropriate rehabilitation projects. Assessing pavement conditions is an essential first step in this process. This asphalt pavement surface condition rating procedure has
proven effective in improving decision making and using funds more efficiently. It can be used directly by airport staff and consultants. It may be combined with additional testing and data collection in a more comprehensive pavement management system.
Practical advice on rating airfield pavement 24
A pavement’s ability to carry heavy traffic loads depends on both the pavement materials (asphalt surfacing and granular base) and the strength of the underlying soils. Most soils lose strength when they are very wet. Therefore, it is important to provide drainage to the top layer of the subgrade supporting the pavement structure.
Planning annual maintenance and repair budgets
We have found that relating a normal maintenance or rehabilitation procedure to the surface rating scheme helps managers use the rating system. However, an individual surface rating should not automatically dictate the final maintenance or rehabilitation
References
Concrete Aviation Airfields PASER Manual, 2003, Engineering Professional Development, College of Engineering, University of Wisconsin-Madison.
Guidelines and Procedures for Maintenance of Airport Pavements, 7/14/03, Federal Aviation Administration, Advisory Circular AC:150/5380-6A.
AIRFIELD PAVEMENT INVENTORY
AIRFIELD PAVEMENT INVENTORY
Airfield … Condition survey date …
Done by …
Facility (runway, taxiway, apron) …
Feature description …
Feature location …
Feature area …
Construction date …
Pavement type: ■Asphalt ■Concrete Layer thicknesses: … … …
Maintenance history …
…
…
PASER Rating ( 5 = Excellent, 4 = Good, 3 = Fair, 2 = Poor, 1 = Failed) ■
Comments on pavement and drainage conditions …
…
…
…
…
Recommended maintenance …
…
…
…
…
Recommended rehabilitation …
…
…
…
PASER
Asphalt Airfield Pavements
AC 150/5320-17 Appendix 2 7/12/2004
APPENDIX 2--CONCRETE AIRFIELD PAVEMENT
APPENDIX 2--CONCRETE AIRFIELD PAVEMENT
SURFACE EVALUATION AND RATING MANUAL
Pavement Surface Evaluation and Rating PASER Manual
Concrete Airfield Pavements
RATING
5
RATING
3
RATING
1
This manual is intended to assist airfield managers in understanding and rating the surface condition of rigid Portland Cement Concrete (PCC) pavements. It describes types and causes of distress and provides a simple system to visually rate pavement condition.
SURFACE EVALUATION AND RATING MANUAL
Produced for the Federal Aviation Administration by Engineering Professional Development, College of Engineering, University of Wisconsin-Madison.
Contents
Introduction 2
Evaluating pavement condition 3
Surface defects 4
Joints 6
Pavement cracks 7
Pavement distortion 10
Rating pavement surface condition 13
Rating system 13
Rating 5 — Excellent 14
Rating 4 — Good 14
Rating 3 — Fair 15
Rating 2 — Poor 16
Rating 1 — Failed 17
Practical advice on rating roads 19
Airfield Pavement Inventory inside back cover
Donald Walker, P.E., University of Wisconsin–Madison, author Lynn Entine, Entine & Associates, editor Susan Kummer, Artifax, designer
PASER Manual
Pavement Surface Evaluation and Rating
Concrete Airfield Pavements
An airport manager’s goal is to use available funds to provide a safe and economical pavement surface. This is no simple task. It requires balancing priorities and making difficult decisions in order to manage pavements. This manual offers useful information for planning maintenance and managing Portland Cement Concrete (PCC) pavements. It discusses common problems and typical repairs and includes a visual system for evaluating and rating PCC pavements.
General aviation airfield pavements are often managed informally, based on the staff’s judgment and experience. While this process is both important and functional, using a slightly more formalized technique can make it easier to manage pavements effectively.
Experience has shown that there are three steps that are especially useful in managing airfield pavements:
1) Inventory all pavements.
2) Periodically evaluate the condition of all pavements.
3) Use the condition evaluations to set priorities for projects and evaluate alternative treatments.
A comprehensive pavement management system involves collecting data and assessing several pavement characteristics: roughness, surface distress (condition), surface skid characteristics, drainage, and structure (pavement strength and deflection). Planners can combine this condition data with economic analysis, to develop short-range and long-range plans for a variety of budget levels. However, general aviation agencies may lack the resources for such a full-scale system.
Since surface condition is the most vital element in any pavement management system, managers may use the simplified rating system presented in this Concrete Airfield Pavements PASER Manual to evaluate their pavements. A PASER Manual for asphalt airfield pavements is also available (see References, page 20).
PASER — Pavement Surface Evaluation and Rating Concrete Airfield Pavements
Rigid pavement performance
PCC pavements are either plain (nonreinforced) or reinforced concrete. Reinforcement is usually provided by steel wire mesh placed approximately at mid-slab depth. The reinforcement is intended to limit crack opening and movement in the concrete slab. Most airfield pavements are not reinforced.
Since concrete slabs need to move (expand and contract) with changes in temperature and during initial cure (drying and shrinkage), pavements are constructed with contraction joints. These are usually sawn into the pavement shortly after initial curing. This joint gives the slab a place to crack and makes a straight, well-formed groove to seal. Runways, taxiways and aprons (ramps) are sawn to create square slabs ranging from 15’ to a maximum of 25’.
Isolation joints are occasionally provided. These are wider, full depth, and filled with a material to allow expansion. If used, they are placed adjacent to structures that cannot move with the pavement such as buildings, manholes, and other utility structures. These isolation joints are also used at pavement intersections and allow changes in joint patterns.
Rigid, PCC pavements carry traffic loadings differently than flexible pavements (asphalt). Concrete pavements are designed to act like a beam and use the bending strength of the slabs to carry the load. Therefore, load transfer across cracks and joints is important, especially on pavements with heavy traffic loading. Hairline and narrow cracks still have interlocked concrete aggregate and can effectively transfer loads. Because wide cracks and widely-spaced joints open up, they cannot transfer loads and must take
Evaluating pavement condition
higher edge loads. These higher edge loads can cause further cracking and deterioration along the joint, or crack edges.
Many concrete pavements use joints that have load transfer dowels. These are smooth steel bars placed across the joint. They transfer traffic loads between adjacent concrete slabs while allowing the joint to open and close. These bars can rust and sometimes cause problems. The corrosion causes forces on the concrete which leads to spalling, cracking, and general joint deterioration. Epoxy coated dowels may be used to reduce corrosion.
Unsupported slab edges will deflect or bend under a load. If the supporting soil is saturated it can squirt up through joints or cracks when the slab bends. This is called pumping. Eventually the loss of supporting soil through pumping creates an empty space or void under the slab. The slabs may then crack further under loads and joints will deteriorate more.
Undoweled joints under heavy traffic may fault. This is when one slab edge is lower than the next slab. Faulting is more likely on pavements with most of the traffic in one direction. The downstream traffic slab will be lower than the upstream slab, creating a step. Faulting creates a rough pavement.
You can often detect pumping by the soil stains around pavement joints or cracks. The resulting voids can be grouted full or sub-sealed. Slabs can be leveled by slab jacking or mud jacking. Obviously, sealing cracks and joints and improving subsoil drainage will help reduce pumping, faulting, and joint failures.
PCC pavement conditions and defects
It is helpful to separate various conditions common to PCC pavements. These are described individually in some detail. We include causes for deterioration and common strategies for repair. Some defects are localized while others indicate that problems may develop throughout the pavement. It is important to distinguish between local and widespread defects. Assessing the conditions of actual pavements also involves looking for combinations of these individual defects.
There are four major categories of common PCC pavement surface distress and condition:
Surface defects Polishing, map cracking, pop-outs, scaling, spalling.
Joints Longitudinal and transverse joints.
Pavement cracks Slab cracks, D-cracking, corner cracks, meander cracks, manhole and inlet cracking.
Pavement distortion Pavement settlement or heave; blow ups; faulting; utility repairs, patches and potholes.
In reviewing the different defects it is important to consider both their severity and extent. Generally, conditions begin slowly and progressively become more serious. Slight defects may grow into moderate and then severe conditions. In addition, defects might initially be indicated only in a few isolated cases. Examples in the rating section will help identify how bad and how extensive a condition is.
EVALUATION — Surface Defects 4
SURFACE DEFECTS
SURFACE DEFECTS
Polishing
A worn or polished surface may develop from traffic wearing off the surface mortar and skid-resistant texture. An asphalt overlay or grinding the concrete surface can restore skid resistance.
Map cracking
A pattern of fine cracks usually spaced within several inches is called map cracking. It usually develops into square or other geometrical patterns. Map cracking can be caused by improper cure or overworking the surface during finishing. It may also indicate a problem with the quality of the aggregate known as ASR (alkali-silica reactivity). If severe, cracks may spall or the surface may scale. Repair is usually limited to very severe conditions. An asphalt overlay or partial depth patching may then be necessary.
Pop-outs
Individual pieces of large aggregate may pop out of the surface. This is often caused by chert or other absorbent aggregates that deteriorate under freeze-thaw conditions. Pop-outs alone do not usually affect pavement serviceability. However, damage to aircraft from the debris may occur. For severe areas, a patch, overlay or slab replacement may be necessary.
▼ ▼
Extensive
pop-outs
of large aggregate from surface.
Several pop-outs
in a new
slab.
▼
Map cracking
has hairline surface cracks,
probably shallow in depth. May not cause any
long-term performance
problems.
▼
Close-up of a polished
pavement surface.
EVALUATION — Surface Defects 5
Scaling
Scaling is surface deterioration that causes loss of fine aggregate and mortar. More extensive scaling can result in loss of large aggregate. The cause often is using concrete which has not been air-entrained, making the surface susceptible to freeze-thaw damage.
Scaling can occur as a general condition over a large area or be isolated to locations where poor quality concrete or improper finishing techniques caused loss of entrained air. In severe cases, deterioration can extend deep into the concrete. Debris from scaling can damage aircraft.
Grinding may remove poor quality surface concrete. Partial depth patching of isolated areas may also prolong the life of the pavement. Severe scaling may require slab replacement.
Spalling
Spalling is the loss of a piece of the concrete pavement from the surface or along the edges of cracks and joints. Cracking or freeze-thaw action may break the concrete loose, or spalling may be caused by poor quality materials. Spalling may be limited to small pieces in isolated areas or be quite deep and extensive. Large pieces of loose concrete can cause serious damage to aircraft.
Repair will depend on the cause. Small spalled areas are often patched. Spalling at joints may require full depth joint repair or full slab replacement.
Slight scaling. Minor loss of surface mortar.
Moderate surface
scaling. Loss of mortar and fines starting to expose
larger aggregate.
Severe scaling. Some larger aggregate is loose.
▼
▼
▼
Small surface spall that has been patched.
▼
Spall at crack. Creates dangerous debris.
▼
Spalling along a joint.
▼
EVALUATION — Joints 6
JOINTS
Construction joints or sawn joints are narrow and usually well sealed. As pavements age and materials deteriorate, joints may open wider and deteriorate further. Cracks parallel to the initial joint may develop and accelerate into spalling or raveling. Settlement, instability, or pumping of subgrade soil can cause joints to fault. One common cause of cracks parallel to joints is waiting too long after the pour to saw the joint. Then, during initial cure the slab will crack near the sawn joint.
Maintaining a tight joint seal can prevent intrusion of water and debris and reduce freeze-thaw damage and pumping. Debris may accumulate in open joints which prevents normal joint movement. This will greatly accelerate joint deterioration. Severe joint deterioration may require full depth patching and joint replacement.
Taxiway with
spalled joint.
Joint sealant in poor condition. Loss of bond to edge allows water into pavement.
New pavement with good joints.
▼
Joint sealant deterioration on apron. Slab is in good condition.
▼
▼
Severe spalling along joint and crack. Creates debris.
▼
▼
EVALUATION — Cracks 7
PAVEMENT CRACKS
PAVEMENT CRACKS
Slab cracks
Slab cracks divide the slab into 2 or more pieces. They can be caused by thermal stresses, poor subgrade support, or heavy loadings. They are sometimes related to slabs with joints spaced too widely. Slabs with a length-to-width ratio greater than 1.25 are more likely to develop mid-slab cracks.
As with joints, these cracks may deteriorate further if not sealed well. Slabs can fault at cracks. Cracks can spall and develop additional parallel cracking. Severe deterioration may require patching individual cracks. Multiple transverse cracks in individual slabs indicate further deterioration. Extensive slab cracking indicates pavement failure and the need for complete replacement.
Crack next to joint often caused by late sawing. Crack shows early signs of spalling.
Hairline slab crack. Tight with no spalling.
▼
▼
Slab crack with grass, no sealant, and spalls developing.
▼
▼
Slab crack with spalling and debris.
▼
Multiple slab cracks and broken pavement. Replacement needed.
▼
Closely spaced, hair-line, transverse cracks indicate slab is broken and needs replacing.
▼
EVALUATION — Cracks 8
D-cracks
Occasionally, severe deterioration may develop from poor quality aggregate. So called D-cracks or disintegration cracking, develop when the aggregate is able to absorb moisture. This causes the aggregate to break apart under freeze-thaw action which leads to deterioration. Usually, it starts at the bottom of the slab and moves upward.
Fine cracking and a dark discoloration adjacent to the joint often indicate a D-cracking problem. Once this is visible on the surface the pavement material is usually severely deteriorated and complete replacement is required.
Joint or crack sealing helps slow D-cracking deterioration. This is a serious defect because it may indicate a material quality problem throughout the pavement. Milling and patching has proven successful as a short term repair.
Corner cracks
Diagonal cracks may develop near the corner of a concrete slab, forming a triangle with the joint. Usually these cracks are within a foot or two of the slab corner and are caused by insufficient soil support or concentrated stress due to temperature-related slab movement. The corner breaks under traffic loading. They may begin as hairline cracks.
Some corner cracks extend the full depth of the slab while others start at the surface and angle down toward the joint. With further deterioration, more cracking develops, and eventually the entire broken area may come loose. This may be a localized failure, but it often indicates widespread maintenance problems.
Partial or full depth concrete patching or full depth joint replacement may be needed when corner cracking is extensive.
Surface discoloration near joints and cracks indicates D-cracking and severe slab deterioration.
Multiple crack patterns adjacent to joints. Common D-cracking pattern.
▼
Corner cracking in
all four slabs.
▼
Corner cracking
with slight spalling.
▼
Corner cracking,
severe spalling,
and dangerous
debris.
▼
▼
▼
EVALUATION — Cracks 9
Meander cracks
Some pavement cracks appear to wander randomly. They may cross a slab diagonally or meander in a random manner. Meander cracks may be caused by settlement due to unstable subsoil or drainage problems. Frost heave and spring thaw can also cause them. They are often local in nature and may not indicate general pavement problems.
Minor cracks may benefit from sealing to minimize water intrusion. Extensive or severe meander cracks may require replacing the slab, stabilizing the subsurface, or improving drainage.
Manhole and inlet cracks
The pavement adjacent to a light can, manhole, or storm sewer inlet often cannot accommodate normal pavement movement due to frost heaving and temperature changes. Cracks and faulting may develop and the concrete slab may deteriorate further. These are often localized design defects that may not indicate a general pavement problem. Sealing and patching may slow the deterioration. Eventually full depth repairs may be required.
Inlet with severe
cracking and spalling. Full depth slab repair required.
▼
Slabs replaced next to inlet. Good joint design.
▼
Meander crack caused by settlement. Lack of maintenance allows water to intrude and debris to collect in crack.
▼
Faulting and spalling of a meander crack.
▼
Two spalls at manhole in a new pavement. Partial depth patching would be beneficial. ▼
PAVEMENT DISTORTION
PAVEMENT DISTORTION
Pavement settling or heave
Unstable or poorly drained subgrade soils may cause pavements to settle after construction. Poorly compacted utility trenches may also settle. This may be a gentle swale or a fairly severe dip.
Frost-susceptible soils and high water tables can cause pavements to heave during the winter months. Extensive pavement cracking and loss of strength during the spring can result in severe deterioration. Improved drainage and stabilization of subgrade soils is usually necessary, along with pavement reconstruction.
Blowups
Concrete slabs may push up or be crushed at a joint. This is caused by expansion of the concrete where incompressible materials (sand, debris, etc.) have infiltrated into poorly sealed joints. As a result, there is no space to accommodate expansion. It is more common in older pavements with long joint spacing. Pavements that have aggregate susceptible to ASR may experience more frequent blowups. Pressure relief joints can be installed and blowup areas must be patched or reconstructed. Cleaning and sealing joints will help prevent blowups.
Internal pressure has partially raised slab at the joint. Complete replacement is required.
Settlement caused meander crack with faulting.
▼
Extensive cracking and patching caused by settlement. Pavement was built on unstable sub-grade soils. ▼
Pavement blowup in progress— concrete is crushed and slab buckled. ▼
▼
EVALUATION — Distortion 10
EVALUATION — Distortion 11
Faulting
Joints and cracks may fault or develop a step between adjacent slabs. Faulting is caused by pumping of subgrade soils and creation of voids. Heavy traffic can rapidly accelerate faulting. Joints may fault due to settlement of an adjacent slab.
Faulting creates a rough pavement and may cause slab deterioration. Minor faulting can be corrected by surface grinding. Voids can be subsealed, or slabs can be mud jacked back to level position. Severe cases may need joint or slab replacement. Faulting of joints. Aggravated by heavy traffic in one direction. Could improve surface by grinding.
▼
Severe joint fault
and spalling.
Severe joint fault.
▼
▼
EVALUATION — Distortion 12
Utility repairs, patches and potholes
Slab replacement or repair of utilities will require cuts and slab patching. Patches from previous repairs may perform like original pavement or may show settlement, joint deterioration or distress.
Localized failures of materials or subgrade soil can cause individual potholes. Surface spalling or other material defects may develop into localized potholes. Full depth patching or slab replacement is usually required.
Full depth joint repair. Very good
condition.
▼
Partial depth concrete patch to repair corner
cracks. Good
condition.
Joint repair with asphalt.
Very good condition.
▼
Potholes caused
by severe joint
deterioration.
Need repair.
▼
Asphalt patches. Poor (top) and fair (bottom) condition.
▼ ▼
Using your understanding of pavement conditions and distress, you can evaluate and rate airfield PCC pavements. The rating scale ranges from 5–excellent condition to 1–very poor or failed. Some pavements will deteriorate through the phases listed in the rating scale. The time it takes to go from an excellent (5) to failed condition (1) depends largely on the quality of the original construction, age, and the amount of heavy traffic loading.
Once significant deterioration begins, it is common to see pavements deteriorate rapidly. This is usually due to the combined effects of loading and additional moisture. As a pavement ages and additional cracks develop, more moisture can enter and accelerate the rate of deterioration.
Rating system
Rating pavement surface condition
Surface rating
Visible distress* General condition/ treatment measures
None. 5 Excellent
Hairline or sealed cracks 1⁄8” wide or less. Map cracking. Pop-outs. 4 Good
Several slabs broken into two pieces by slab cracks. Corner cracking on several slabs, 1⁄4” wide with no spalling. Joint sealant mostly in good condition, less than 10% needing replacement. Several patches in fair to good condition. Map cracking or scaling on 10% or less of the surface area. Slight faulting, less than 1⁄4”, in several locations.
3 Fair
3 Fair
Many slab cracks, some breaking the slab into three or more pieces. Cracks open 1⁄8” or cracks with spalling. D-cracks at several joints. Sealant failure over 10% of joints. Several patches in fair to poor condition with cracks in patch and uneven surface. Faulting 1⁄4” to 1⁄2” in several locations. Severe or extensive scaling.
2 Poor
2 Poor
Many wide cracks with failed sealant and grass. Extensive crack and joint spalling. Slabs extensively cracked or shattered. Many corner breaks with spalling. D-cracks with spalling. Patches in poor condition with spalling. Numerous faults over 1⁄2”.
New pavement or recent major concrete rehabilitation. Like-new condition. Less than 5 years old. No maintenance required.
Concrete over 5 years old. Signs of wear. Minor spot repair of cracks or joint sealant.
First sign of significant slab cracking, corner cracking, scaling, or faulting. Several patches. Joint sealant repair required. Isolated repair of joint or patch.
Needs sealant replacement on more than 10% of cracks or joints. Partial depth or full depth joint repairs or patch replacement. Repair faulted joints. Replace or overlay slabs with severe scaling. Bonded or unbonded concrete overlay.
Extensive full depth joint repairs or slab replacements. Extensive patching and complete overlay. Complete reconstruction. 1 Failed
* A given pavement segment may not have all of the types of distress listed for a particular rating. It may have only one or two types.
Look at the photographs which follow and become familiar with the descriptions of the individual rating categories. To evaluate an individual pavement, first determine its general condition. Is it relatively new, toward the top end of the scale? In very poor condition and at the bottom of the scale? Or somewhere in between? Next, think generally about the appropriate maintenance method.
Finally, review the individual pavement condition and distress and select the appropriate pavement surface rating. Individual pavements may not have all of the types of distress listed for any particular rating. They may have only one or two types. Use the categories in the rating table below.
Each rating also includes a recommendation for needed maintenance or repair. This makes the rating system easier to use and enhances its value as a tool in ongoing airfield pavement maintenance.
Rating 5 – Excellent No maintenance required.
Rating 4 – Good Minor routine maintenance, crack or joint sealing.
Rating 3 – Fair More crack or joint sealing. Isolated joint repairs or slab patching.
Rating 2 – Poor Extensive crack or joint sealing. Repair severe joint deterioration. Partial and full-depth slab repairs.
Rating 1 – Failed Reconstruction.
Rating pavement surface condition 14
RATING 5
RATING 5
EXCELLENT — No maintenance required
Rating 5 is for new pavement or for recent major concrete rehabilitation. Like-new condition. Less than 5 years old. No maintenance required.
New or like-new pavement condition.
▼
▼
RATING 4
GOOD — Little or no maintenance required
Minor spot repair of cracks or joint sealing required. PCC pavement over 5 years old. Signs of wear: hairline or sealed cracks 1⁄8” wide or less, map cracking, pop-outs.
RATING 4
Surface wear and pop-outs.
Partial loss of joint sealant.
▼
Map cracking, but pavement is sound.
Isolated meander crack, tight and well sealed.
▼
▼
Rating pavement surface condition 15
RATING 3
FAIR — First sign of significant slab cracking, corner cracking, scaling, or faulting. Several patches. Joint sealant repair required. Isolated repair of joint or patch.
RATING 3
Several slabs broken into two pieces by slab cracks. Corner cracking on several slabs, 1⁄4” wide with no spalling. Joint sealant mostly in good condition, less than 10% needing replacement. Several patches in fair to good condition. Map cracking or scaling on 10% or less of the surface area. Slight faulting, less than 1⁄4”, in several locations.
Crack breaks slab into two pieces. Well sealed.
Crack breaks off large corner of slab.
▼
Crack parallel to joint. Open 1⁄4”. No spalling.
▼
▼
Severe scaling. Joint and sealant in fair condition.
▼
Isolated spall at manhole.
▼
Moderate scaling.
▼
Rating pavement surface condition 16
RATING 2
RATING 2
POOR —Cracks open 1/8”, D-cracks at joints. Replace sealant, repair joints.
Many slab cracks, some breaking the slab into three or more pieces. Cracks open 1/8” or cracks with spalling. D-cracks at several joints. Sealant failure over 10% of joints. Several patches in fair to poor condition with cracks in patch and uneven surface. Faulting 1/4” to 1/2” in several locations. Severe or extensive scaling.
Open joint
with spalling.
Corner cracks with spalling.
Full depth patch required.
Open cracks with edge spalling. Corner crack and broken corner piece.
Open joints and cracks. Need sealant on more than 10% of joints.
Full depth joint repair required.
▼
Concrete patch in poor condition.
▼
▼
▼
▼
Faulting of joints aggravated by heavy traffic in one direction.
▼
▼
Rating pavement surface condition 17
▼
Severe joint fault
and spalling.
▼
RATING 1
RATING 1
FAILED — Extensive repairs, overlay, or complete reconstruction necessary.
Many wide cracks with failed sealant and grass. Extensive crack and joint spalling. Slabs extensively cracked or shattered. Many corner breaks with spalling. D-cracks with spalling. Patches in poor condition with spalling. Numerous faults over 1⁄2”. Extensive full depth joint repairs or slab replacements, extensive patching and complete overlay, or complete reconstruction needed.
Multiple slab cracks, spalling and shattered slabs.
Failed joint with severe spalling and pothole.
▼
▼
Inlet with severe cracking and spalling. Full depth slab repair required.
Rating pavement surface condition 18
RATING 1
FAILED (continued)
Severe scaling over
extensive areas.
Reconstruction
required.
▼
Closely spaced cracks
and poor
joint. Reconstruct.
▼
Severe deterioration.
Requires reconstruction.
▼
Inventory and field inspection
Most airport owners routinely observe pavement conditions as a part of their normal work. However, an actual inspection means looking at the entire system as a whole and preparing a written summary of conditions. This inspection has many benefits over casual observations. It can be helpful to compare pavement features, and ratings decisions are likely to be more consistent because the system is considered as a whole within a relatively short time.
An inspection also encourages a review of specific conditions important in pavement maintenance, such as drainage, adequate strength, and safety.
A simple written inventory is useful in making decisions where other people are involved. You do not have to trust your memory, and you can usually answer questions in more detail. Having a written record and objective information also improves your credibility with the funding agencies.
Finally, a written inventory is very useful in documenting changing pavement conditions. Without records over several years, it is more difficult to know if conditions are improving, holding their own, or declining.
A sample inventory form is shown on the inside back cover. It is very helpful to collect background information on each feature. Pavement thickness, age, and major maintenance are examples of helpful information.
Annual budgets and long range planning are best done when based on actual needs as documented with a written inventory.
Pavement features
Inventory and pavement condition data are normally organized by dividing the pavements into segments or features. A plan or aerial photo of the entire airfield is most helpful in identifying these
individual features. Runways, taxiways and aprons should be considered as separate categories. Within each category, the pavement should be separated into features with similar construction. For example, pavements with different thickness, age, or type of construction should be rated separately.
A runway may be all one feature if conditions are similar. However, if parts of the runway have significantly different construction details or condition, then separate features will make the rating more logical and useful.
Each taxiway, can be considered a separate feature. You may combine several sections of taxiway if conditions are similar.
Apron areas can be separated into features according to the areas they serve. For example, aprons serving a terminal, hangers, tie-down area, or fueling area would be separate features. Areas in different conditions may also be separated into features.
It is helpful to note the size of slabs or panels as well as the number of slabs in a feature. The overall area can be calculated and used to prepare maintenance or construction estimates.
Averaging and comparing sections
No pavement feature is entirely consistent. Also surfaces in one section may not have all of the types of distress listed for any particular rating. They may have only one or two types.
The objective is to rate the condition that represents the majority of the pavement feature. Small or isolated conditions should not influence the rating. It is useful to note these special conditions on the inventory form so this information can be used in planning specific improvement projects. For example, some spot repairs may be required.
Occasionally surface conditions vary significantly within a feature. For example, short sections of good condition may be followed by sections of poor surface conditions. In these cases, it is best to rate the feature according to the worst conditions and note the variation on the form.
The overall purpose of condition rating is to be able to compare each feature relative to all the other features in your airport pavement system. On completion you should be able to look at any two pavement features and find that the better surface has a higher rating.
Assessing drainage conditions
Moisture and poor pavement drainage are significant factors in pavement deterioration. Some assessment of drainage conditions during pavement rating is highly recommended. While you should review drainage in detail at the project level, at this stage simply include an overview drainage evaluation at the same time as you evaluate surface condition.
Consider both pavement surface drainage and lateral drainage (ditches or storm sewers). Pavement should be able to quickly shed water off the surface. Ditches should be large and deep enough to drain the pavement and remove the surface water efficiently into adjacent waterways.
Look at the crown and check for low surface areas that permit ponding. Runways and taxiways should have approximately a 1.5º% cross slope or crown across the pavement. Apron areas require positive drainage and often include storm drainage systems. Maintenance of the entire drainage system is critical. Ditches, subsurface drains and outlets should be inspected
Practical advice on rating airfield pavements
Practical advice on rating airfield pavements 20
managers use the rating system. However, an individual surface rating should not automatically dictate the final maintenance or rehabilitation technique.
Consider future traffic projections, original construction, and pavement strength since these may dictate a more comprehensive rehabilitation than the rating suggests.
Summary
Using funds most efficiently requires good planning and accurate identifi-
and cleaned regularly.
A pavement’s ability to carry heavy traffic loads depends on both the pavement materials (concrete slab and granular base) and the strength of the underlying soils. Most soils lose strength when they are very wet. Therefore, it is important to provide drainage to the top layer of the subgrade supporting the pavement structure.
Planning annual maintenance and repair budgets
We have found that relating a normal maintenance or rehabilitation procedure to the surface rating scheme helps
cation of appropriate rehabilitation projects. Assessing pavement conditions is an essential first step in this process. This pavement surface condition rating procedure has proven effective in improving decision making and using funds more efficiently. It can be used directly by airport staff and consultants or combined with additional testing and data collection in a more comprehensive pavement management system.
References
Asphalt Airfield Pavements PASER Manual, 2003, Engineering Professional Development, College of Engineering, University of Wisconsin-Madison.
Guidelines and Procedures for Maintenance of Airport Pavements, 7/14/03, Federal Aviation Administration, Advisory Circular AC:150/5380-6A.
AIRFIELD PAVEMENT INVENTORY
AIRFIELD PAVEMENT INVENTORY
Airfield … Condition survey date …
Done by …
Facility (runway, taxiway, apron) …
Feature description …
Feature location …
Feature area …
Construction date …
Pavement type: ■Asphalt ■Concrete Layer thicknesses: … … …
Maintenance history …
…
…
PASER Rating ( 5 = Excellent, 4 = Good, 3 = Fair, 2 = Poor, 1 = Failed) ■
Comments on pavement and drainage conditions …
…
…
…
Recommended maintenance …
…
…
…
…
Recommended rehabilitation …
…
…
…
PASER